Corrosion is a costly and potentially life threatening problem in any industry.
Wherever there is metal the potential for a corrosive reaction exists. It is a natural part of
nature, there is no escaping it. That doesn’t mean that we are doomed though. Through a
careful analysis of the process and the design we can mitigate most of the costs of
corrosion, both actual and potential, before the first pipe is in place.
The science of corrosion engineering is viewed by many as magic, or art, but once
the basics of how a corrosion cell works and a little understanding of chemistry almost
anyone can learn to decipher the clues to the causes of a corrosion problem. Most
corrosion problems encountered fall into five basic categories:
• Uniform or general corrosion: this is the most common form of
corrosion encountered.
• Localized corrosion: as the name implies this form of corrosion occurs
in discreet areas on the surface of the metal.
• Metallurgically induced corrosion: this form of corrosion attacks the
metal’s physical and chemical makeup.
• Mechanically assisted corrosion: the physical parameters of the system
play an important part in this form of corrosion.
• Stress corrosion cracking: this form of corrosion results in cracks in
the metal that are induced by both stresses and corrosive elements.
With this information we can hopefully reduce the costs of replacing expensive assets
before they have fully depreciated, but our ultimate goal is to reduce the chances of a
catastrophic failure or loss of life due to a corroded system.
Thermodynamic and Electrochemical Processes
The corrosion process of metals is a natural result of the inherent tendency to
revert to a more stable compound, such as an oxide. Metal ore that is mined must be
refined and then alloyed for use. Energy is required to refine these ores into useable
metals. Entropy, a thermodynamic property, drives these metals to corrode. “Every
system which is left to itself will, on the average, change toward a condition of maximum
probability.” (G. N. Lewis) Energy is required to keep these metals in the refined state
and when left alone they will, over time, revert back to the more stable compounds in
which they occur naturally.
An example of this is iron. Hematite is the principle ore of iron. Hematite is a
form of iron oxide, its chemical composition is FE2O3. Processed iron ore, coke, and
limestone are added to the top of a blast furnace (Figure 1-1).1
The coke is the source of
the chemical energy in the blast furnace. When it is burnt by the hot air it releases both
heat energy and the main reducing agent, CO.
2C + O2
∆H
2CO ∆H = -394 kJ/mol
The limestone is decomposed by the heat into calcium oxide, CaO, and additional
carbon monoxide.
2CaCO3
∆H
2CaO + 2CO + O2
The main chemical reaction takes place, and the calcium oxide combines with the
impurities in the ore to form slag.
Fe2O3 + 3CO ∆H
3CO2 + 2Fe
The refined iron then runs down and out of the blast furnace to form pig iron. The
pig iron is then combined with other alloys to get different kinds of steels.
1
U.S. Department of Energy's Office of Fossil Energy website (December 14, 2001).
Figure 1-1. The blast
furnace is used to turn
iron ore into pig iron for
the steel making process.
At this point, the second law of thermodynamics and free energy come into play.
The second law of thermodynamics quite simply states: “The stable, equilibrium state of
a system is the state of minimum free energy.”2
Iron in the processed form, Fe, has a
greater amount of free energy than iron oxide. That energy was added when the ore was
heated in the blast furnace. The system, in this case the processed iron, will always be
headed towards its most stable state, which is the state of minimum free energy. When
moisture and oxygen are present the iron will undergo a chemical reaction to reduce the
amount of free energy available. This redox, reduction oxidation, reaction produces
hydrated iron oxide:
4Fe+2
(aq) + O2(g) + [(4 + 2x)H2O](l) [2Fe2O3 · xH2O](s) + 8H+
(aq)
The resulting iron oxide, Fe2O3, is one of the most stable states for iron to be found in.
This simple example of an electrochemical reaction demonstrates one of the most
important principles of metallic corrosion: the rate of oxidation equals the rate of
reduction.3
It is important to note that when alloys are corroded more than one oxidation
and one reduction reaction can occur.
Another way of looking at the corrosion process is as a series of anodic and
cathodic reactions. In this situation four elements are necessary for corrosion to occur:
• An anode.
• A cathode.
• An electrolyte (water)
• A metallic path for electron flow.
When all four of these elements are present a corrosion cell is formed. It is
important to remember that the anodic and cathodic reactions do not have to occur at the
same spot on the material. As long as an electrolyte and a metallic path exist, these half-
cells can exist and corrosion will occur. Figure 1-2 is an example of the corrosion cell
with the four elements labeled.4
2
Davis, Neil T. (2001) page 37.
3
Fontana, Mars G. (1986) page 15.
4
Allen, Thomas O., Roberts, Alan P. (1993) page 10-1, 10-2.
Figure 1-2. Corrosion
cell diagram depicting
the current flow from the
corrosion pit.
The same redox reactions that occurred in the afore mentioned example are
occurring in the corrosion cell. The oxidation reaction takes place at the anode, and the
reduction reaction takes place at the cathode. It is this series of oxidation and reduction
reactions that make up the electrochemistry of the corrosion process.
It is important to note that there is a flow of electrons from one half-cell to the
other during the corrosion process. The electric current flows from the anodes to the
cathodes of the reaction through the electrolyte. The flow of electric current in the
corrosion cell per unit area is referred to as the Corrosion Current Density (icorr). As each
oxidation reaction occurs a transfer of electrons to the electrolyte occurs. Since icorr is a
measure of current flow per unit area per unit time it can be seen that icorr can be related to
units of metal loss per unit time. Corrosion rates are generally expressed in mils per year
of metal thickness reduction (MPY), so icorr is a good representative of the corrosion rate
in the cell.5
Armed with this information it is possible to slow down or even prevent the
corrosion from occurring by increasing the resistance in the electrochemical corrosion
circuit. Adding chemical inhibitors and coatings to the materials to reduce the current
flow will help to increase the circuit resistance.
The free energy available in the metal and in the electrolyte creates a potential at
the anode and at the cathode. It is the difference in potential between these two sites that
causes the electron flow. Most corrosion reactions are considered wet and occur in the
presence of a liquid. Marcel Pourbiax, a well-known Belgian scientist, developed a
diagram which relates the stability of a metal in a given pH environment in 1938. By
plotting the potential of a metal and the pH of the environment it is possible to determine
if the metal is in a region where the possibility of corrosion is high, the possibility for
corrosion is non-existent, or the possibility exists but there is a tendency for the
development of a protective film. Figure 1-3 is the Pourbiax diagram for an iron-water
system at 25 degrees Celsius.6
The gray zone represents the area where the base metal,
iron, is stable. This is the region where the possibility of corrosion is non-existent. The
orange zone is where rust, the non-protective form of corroded iron, is expected. The
blue zone is where the most stable iron species, Fe(OH)2, is encountered. This species is
called blue rust and is fairly rare and highly soluble. The white areas are where corrosion
is most probable.
5
Rohrback Casaco Systems website (December 14, 2001) page 3.
6
Corrosion Doctors website (December 13, 2001).
Figure 1-3. Pourbiax diagram for an
iron-water system at 25û C.
These Pourbiax diagrams are time consuming to create and a new diagram must
be created for each metal or alloy that is being used and the environment it is in. There
are software programs available that can produce these diagrams for the student of
corrosion processes.7
It is not enough to determine if the possibility for corrosion exists, a corrosion rate
must also be determined. It is entirely possible for the probability of corrosion to be high
and resultant corrosion rates to be very low. In these cases the corrosion might not be a
problem.
Corrosion rates are determined through polarization curves. Polarization curves
are produced through the application of a current to the metal surface. If the potential of
the metal surface is polarized by the current in a positive sense it is referred to as being
anodically polarized; a negative sense signifies that it is cathodically polarized. The
degree of polarization is a measure of how the rates of the anodic and cathodic reactions
are hindered by various environmental and surface process factors. The environmental
factors (the concentrations of metal ions, dissolved oxygen in the solution, etc.) are
referred to as the concentration polarization. The surface process factors (film formation,
adsorption, etc.) are referred to as the activation polarization. The polarization curve is a
graph of the variation of the potential as a function of the current, which allows the
effects of the concentration and activation processes on the rate at which the anodic or
cathodic reactions can give or receive electrons to be determined. This allows for a rate
determination for the reactions that are involved in the corrosion process, in effect a
corrosion rate.8
7
Corrosion Doctors website (December 13, 2001).
8
Encyclopedia of Electrochemistry website (December 13, 2001) page 5.
Figure 1-4. General
Polarization curve for a
material with both anodic
and cathodic polarization
curves.
The polarization curve above shows the polarization curves for both anodic and
cathodic reactions. The potential, E, is plotted as a function of the logarithm of icorr.
Ecorr, the corrosion potential, is determined by the intersection of the extrapolation of the
linear portions of the anodic and cathodic polarization curves. The value of the current at
the intersection is the rate of corrosion expressed in current density, icorr.
From this polarization curve the Evans diagram can be extrapolated. Evans
diagrams are useful in determining if the anodic, cathodic, or both reactions control the
rate of the corrosion. Figure 1-5 shows the three types of Evans diagrams that can be
extrapolated from the polarization curve, (a) shows that the rate is controlled by the
anodic reaction, (b) is controlled by the cathodic reaction, and (c) is controlled by a
combination of both reactions. This information is used by corrosion engineers to allow
the evaluation of the effects of measurable factors, which can be controlled, on the rates
of corrosion.9
Another determining factor in the corrosion rate is the phenomenon of passivity
and passive films. Passivity generally refers to materials that form insoluble films, which
inhibit the anodic reactions and cause a polarization of the anode.10
These films can
markedly reduce the rate of corrosion as long as they are not breached. These films can
experience breakdowns from both electrochemical reactions and mechanical
mechanisms. Those discrete sites where a breach in the film occurs can experience an
accelerated rate of corrosion. One of the major causes of the breaching of the passive
films is the chloride ion, which is readily available in nature.
9
Encyclopedia of Electrochemistry website (December 13, 2001) page 6.
10
Atkinson, J.T.N., Van Droffelaar, H. (1995) page 54.
Figure 1-5. Evans
diagram extrapolated
from the polarization
curve (a) shows that the
rate is controlled by the
anodic reaction, (b) is
controlled by the
cathodic reaction, and (c)
is controlled by a
combination of both
reactions.
An interesting process that some alloys undergo is repassivation. This process is
very effective for combating localized corrosion. These alloys form a passive film that
resists the breakdown process in a fairly effective manor, and are capable of repassivating
at a rate high enough that once a breach has occurred the exposure to the corrosive
environment is reduced to a minimum.11
Forms of Corrosion
From the engineers standpoint the forms that corrosion takes can generally be
identified by a visual examination. It is usually possible to determine a probable
mechanism for the corrosion by corresponding the corrosion in question to one or more
of general forms.
• Uniform or General corrosion: a regular loss of metal from the surface
cases a uniform thinning.
• Localized corrosion: the majority of metal loss is experienced in discrete
areas.
• Metallurgically Induced corrosion
• Mechanically Assisted corrosion: physical environmental factors play a
significant role in metal loss.
• Stress corrosion: generally cracking that is induced by environmental
factors.
These five basic types of corrosion can be broken down into eight visually
identifiable forms, which are significantly different from one another. This allows an
engineer to examine a specimen and make a reasonable assumption on the general cause
of the corrosion and possible corrective measures that can be taken.
General Corrosion
General corrosion, or uniform attack, is the most common form of corrosion.
General corrosion occurs uniformly over the entire surface that is exposed. The metal
gets thinner evenly over the entire surface, leading this form of corrosion to account for
the largest tonnage of metal loss. This form of corrosion is generally the cheapest form
of corrosion to deal with in industry. It is fairly consistent and rates can quickly be found
by exposing a sample to the environment. Making the material thicker than necessary to
accommodate the corrosion throughout the life of the product, or applying a coating to
the surface, such as paint, are the standard methods of prevention for this form of
corrosion.
11
Encyclopedia of Electrochemistry website (December 13, 2001) page 6.
Photo 2-1. Depicts general, or uniform, corrosion on a steel
fitting.
Galvanic Corrosion
Galvanic, or two-metal, corrosion occurs because of the potential difference that
exists between two dissimilar metals. When these two metals can be connected
electrically, either through direct contact or an electrolyte, the difference in potential
causes a flow of electrons, or current, between them. The further apart on the Galvanic
Scale (figure 2-1) that these two metals are increases the amount of corrosion
experienced by anodic member of the galvanic couple. The ensuing corrosion reaction is
a perfect example of the corrosion cell in figure 1-2. The corrosion resistant, or noble,
metal becomes the cathode and experiences very little, if any metal loss. While the less
corrosion resistant metal becomes the anode.
Figure 2-1. The Galvanic Scale.
Photo 2-5. Galvanic corrosion of a bolt.
Photo 2-6. Light galvanic corrosion around a
bolt on a pump housing.
Proper material selection can eliminate most of the problems associated with
galvanic corrosion. Combinations of metals and alloys used together should not be
widely separated on the galvanic scale. Dissimilar metal crevices, such as threaded
connections, should be avoided, and fasteners of the same material or a more noble
material should be used.12
Crevice Corrosion
Crevice corrosion is an intensive, localized form of corrosion. It generally occurs
in cracks, holes, crevices, lap joints, under gaskets, rivet and bolt heads, and anywhere
else that small amounts of solution can lay stagnate. Crevice corrosion begins with the
typical corrosion cell (figure 1-2), an oxygen concentration cell. As the oxygen is
depleted the growth of the corrosion cell is driven by the accumulation of acidic
hydrolyzed salts in the crevice area.
12
Dillon, C.P. (1982) page 47.
Photo 2-7. Galvanic corrosion at the threaded connection between a brass fitting and a
steel backwash line for a water softener.
Photo 2-8. Corrosion of a brass fitting due to
the galvanic couple created with the copper
pipe.
Photo 2-9. Failure due to crevice
corrosion in the threaded area of a
pipe.
Proper material selection and design features that limit the number of crevices and
allow for drainage are the most effective way of mitigating the effects of crevice
corrosion.
Photo 2-10. Excellent example of crevice corrosion on several fronts. Notice the extensive corrosion
between the flange faces, and the corrosion of the bolts that held the flange together.
Photo 2-11. Crevice corrosion is very common in tube and shell heat exchangers. The main
areas of concern are where the tubes enter the tube sheets and where they go through the
baffles. Photo courtesy Tim Milanowski.
Pitting
Pitting is a troublesome form of corrosion. It can cause a failure with very little
metal loss. Pitting is an extremely localized form of attack that often causes rapid
penetration of the wall thickness.13
The holes that pitting causes can be very small or
quite large in diameter. The fact that failure can occur with very little metal loss and with
just one little area affected is what makes this form of corrosion so difficult to detect and
prevent.
13
Dillon, C.P. (1982) page 19.
Photo 2-12. Large pit
that occurred in an oily
water line, this pit had
penetrated about 90% of
the way through the wall.
Photo 2-13. This is an oily water line, and the glycol tracing that was welded to it, that experienced
failure due to pitting. Notice that the pitting occurs on the bottom half of the pipe. Pits usually grow
in the direction of gravity. The largest pits and the failure occurred in the heat-affected zone where
the glycol heat trace was welded to the pipe.
Photos 2-14, 2-15, and 2-16 show how varied small pits can be. In order to detect
that there is a problem you would have to use UT, and be lucky enough to be right on top
of the pit.
Intergranular Corrosion
Intergranular corrosion is the corrosion of the edges of the individual grains that
make up the metal. The preferential attack along the grain boundaries can lead to a
decrease in effective cross section of material and eventual mechanical failure.14
Metals
experiencing intergranular corrosion that should otherwise exhibit excellent corrosion
resistant tendencies have been sensitized. Sensitizing usually occurs through damaging
thermal exposures, such as welding. Material selection, heat-treating, quenching, and
proper welding techniques are effective methods for avoiding intergranular corrosion.
14
Dillon, C.P. (1982) page 89.
Photo 2-14 (upper left). Hole in oily water
line caused by pitting.
Photo 2-15 (upper right). Wormhole pit in
a 1-inch diameter steel water pipe.
Photo 2-16 (left). Failure caused by a
small pit.
Photo 2-17. This is the heat-affected zone from photo 2-13. This is a case of weld
decay in the heat-affected zone.
Selective Leaching
Selective leaching, or dealloying, is the removal of one element from an alloy
through a corrosion process. The most common form of dealloying is the removal of zinc
from brass alloys. Common yellow brass is 30% zinc and 70% copper. The brass turns a
red or copper color that contrasts with the original yellow brass, or zinc oxide builds up
on the outside of the brass piece.
Photo 2-18. Heat-affected zone of a circumferential weld is very distinct in this photo.
Photo 2-21 and Photo 2-22. Dezincification of a brass
valve.
Photo 2-19 and 2-20. Carburization, a special
case of intergranular corrosion. This steel hook
has undergone carburization at high temperatures.
Erosion Corrosion
Erosion corrosion is the accelerated increase in deterioration of a metal due to the
velocity of the fluid. The fluid does not have to contain any abrasive particles, but the
metal will be worn away faster if there are abrasives present.
Photo 2-23. The
velocity effects of
the shell side fluid
in the tube and
shell exchanger
are quite obvious.
Photo courtesy
Tim Milanowski.
Photo 2-24. Hole in the HAZ. This failure was
caused by erosion corrosion. Notice the shape
of the pits, they are deeper on the downstream
side (above the weld line). Here is a good case
of two forms of corrosion working together.
The failure is actually in the heat-affected zone
of the weld, but it is obvious that erosion
played the bigger part in creating the hole itself.
This is from a section of piping just
downstream of a flow meter. In order for the
flow meter to work properly the diameter of the
pipe was reduced several feet upstream of the
meter. This reduction in diameter increased the
velocity through the section of pipe. Photo
courtesy Tim Milanowski.
Photo 2-25. This photo illustrates unique patterns that occur in some of the erosion corrosion cases.
Photo 2-26. Severe erosion
corrosion around a nozzle in
a tube and shell heat
exchanger. Photo courtesy
Tim Milanowski.
Photo 2-27. Severe
erosion corrosion
due to impingement
in a tube and shell
heat exchanger.
Photo courtesy Tim
Milanowski.
Stress Corrosion Cracking
Stress corrosion cracking (SCC) is the cracking from a combined presence of
tensile stresses and a corrosive medium. The tensile stresses can come from applied
stresses or residual stresses. Residual stresses are introduced into a material through
forming, welding, machining, heat treatments, and grinding. The metal remains
unattacked over its surface, while fine cracks progress through it.
Summary
Through a visual examination it is often possible to classify a corrosion problem
by the forms of corrosion that are present. The type of corrosion present tells a lot about
the corrosion mechanisms involved and possible methods to control or alleviate the
Photo 2-28. This is part of a sump float that
exhibits signs of chloride induced stress
corrosion cracking. The cracks are at right
angles to the setscrew, which is where the ring
would experience the greatest stresses.
Photo 2-29. More Chloride
induced stress corrosion
cracking. These two pieces
are from the same sump as
photo 2-28.
corrosion problem. Corrosion can usually be placed in to one or more of the following
visual forms:
• General or Uniform Corrosion.
• Galvanic Corrosion.
• Crevice Corrosion.
• Pitting.
• Intergranular Corrosion.
• Selective Leeching.
• Erosion Corrosion.
• Stress Corrosion Cracking.
Through a careful analysis of the problem a method to avoid any similar problems in the
future can be found. The most important part of any design from the corrosion standpoint
is: Are the materials chosen the right materials for the job, and will they work together?
The Last Exchange. Photo by Tim Milanowski.
References:
About.com Chemistry website (December 4, 2001)
http://chemengineer.about.com/cs/corrosion1/index.htm.
Allen, Thomas O., Roberts, Alan P. (1993) Productions Operations Volume 2 (Oil & Gas
Consultants International, Inc.: Tulsa, Oklahoma).
Alyeska Pipeline Company website (December 12, 2001) http://www.alyeska-
pipe.com/pipelinefacts.html.
Atkinson, J.T.N., Van Droffelaar, H. (1995) Corrosion and Its Control (NACE
International: Houston, Texas).
Boteler, D.H., Seager, W.H., Johanson, C., and Harde, C. (1999) Cold Climate Corrosion
Special Topics: Telluric Current Effects on Long and Short Pipelines (NACE
International: New York, New York) pp 67-79.
Corrosion Doctors website (December 13, 2001) http://www.corrosion-doctors.org.
Corrosion Research Center website (December 1, 2001)
http://www3.cems.umn.edu/research/crc/.
Corrosion Source website (December 4, 2001) http://www.corrosionsource.com.
Corrosion Technology Testbed website (December 11, 2001)
http://corrosion.kcs.nasa.gov/html/crevcor.htm.
Davis, Neil T. (2001) Permafrost A Guide To Frozen Ground in Transition (University of
Alaska Press).
Dillon, C.P. (1982) Forms of Corrosion Recognition and Prevention (NACE
International: Houston, Texas).
Encyclopedia of Electrochemistry website (December 13, 2001)
http://electrochem.cwru.edu/ed/encycl/.
Fontana, Mars G. (1986) Corrosion Engineering (McGraw-Hill, Inc: New York, New
York).
King, R.J., White, W.E. (1999) Cold Climate Corrosion Special Topics: Thermodynamic
Consideration Relevant to Corrosion of Pipeline Steels in Permafrost (NACE
International: New York, New York) pp 37-66.
Korb, Lawrence J., Olson, David L. (1987) Metals Handbook Ninth Edition, Volume 13
Corrosion (ASM International: Houston, Texas).
Milanowski, Tim (December 2001) Inspection Coordinator for Williams Alaska
Petroleum, North Pole, Alaska.
Minnesota Power Electric website (December 12, 2001)
http://www.mpelectric.com/storms/elctrjet.htm.
Moniz, B.J. (1994) Metallurgy (American Technical Publishers, Inc.: Homewood,
Illinois).
Ryan’s Crevice Corrosion Page (December 10, 2001)
http://www.personal.psu.edu/users/r/c/rcw134/crevice.html.
Rohrback Casasco Systems website (December 14, 2001) http://www.corrpro.com/rcs/.
Southwest Research Institute website (December 13, 2001)
http://www.swri.org/3pubs/ttoday/fall96/pipe.htm.
The Hendrix Group website (December 4, 2001) http://www.hghouston.com/tidbits.html.
U.S. Department of Energy’s Office of Fossil Energy website (December 10, 2001)
http://www.lanl.gov/projects/cctc/factsheets/bstel/blastfgrandemo.html.

Mais conteúdo relacionado

Mais procurados

Hydrogen Embrittlement : Causes, Effects, Prevention.
Hydrogen Embrittlement : Causes, Effects, Prevention.Hydrogen Embrittlement : Causes, Effects, Prevention.
Hydrogen Embrittlement : Causes, Effects, Prevention.
Sidheshwar Kumar
 
Corrosion and degradation of materials
Corrosion and degradation of materialsCorrosion and degradation of materials
Corrosion and degradation of materials
Ghassan Alshahiri
 
Chapter5 corrosion
Chapter5 corrosionChapter5 corrosion
Chapter5 corrosion
Wan Zulfadli
 

Mais procurados (20)

Chapter 5 Metal and Imperfections in Solid
Chapter 5 Metal and Imperfections in SolidChapter 5 Metal and Imperfections in Solid
Chapter 5 Metal and Imperfections in Solid
 
Corrosion & its control measures
Corrosion & its control measuresCorrosion & its control measures
Corrosion & its control measures
 
Hydrogen Embrittlement : Causes, Effects, Prevention.
Hydrogen Embrittlement : Causes, Effects, Prevention.Hydrogen Embrittlement : Causes, Effects, Prevention.
Hydrogen Embrittlement : Causes, Effects, Prevention.
 
Corrosion engineering
Corrosion engineeringCorrosion engineering
Corrosion engineering
 
Corrosion control by inhibitor
Corrosion control by inhibitorCorrosion control by inhibitor
Corrosion control by inhibitor
 
Chapter 1 INTRODUCTION TO MATERIAL SCIENCE AND METALLURGY
Chapter 1 INTRODUCTION TO MATERIAL SCIENCE AND METALLURGYChapter 1 INTRODUCTION TO MATERIAL SCIENCE AND METALLURGY
Chapter 1 INTRODUCTION TO MATERIAL SCIENCE AND METALLURGY
 
Corrosion and degradation of materials
Corrosion and degradation of materialsCorrosion and degradation of materials
Corrosion and degradation of materials
 
Principles of corrosion
Principles of corrosionPrinciples of corrosion
Principles of corrosion
 
nucleation and methods to control grain structure
nucleation and methods to control grain structurenucleation and methods to control grain structure
nucleation and methods to control grain structure
 
Chapter 4 Crystal Structures
Chapter 4 Crystal Structures Chapter 4 Crystal Structures
Chapter 4 Crystal Structures
 
Welding of copper alloys
Welding of copper alloysWelding of copper alloys
Welding of copper alloys
 
Chapter5 corrosion
Chapter5 corrosionChapter5 corrosion
Chapter5 corrosion
 
Hydrogen Damage
Hydrogen DamageHydrogen Damage
Hydrogen Damage
 
Corrosion
CorrosionCorrosion
Corrosion
 
Mechanisms of strengthening in metals
Mechanisms of strengthening in metalsMechanisms of strengthening in metals
Mechanisms of strengthening in metals
 
Corrosion control
Corrosion control Corrosion control
Corrosion control
 
Nitriding and carbonitriding copy
Nitriding and carbonitriding   copyNitriding and carbonitriding   copy
Nitriding and carbonitriding copy
 
Introduction to steel making processes
Introduction to steel making processesIntroduction to steel making processes
Introduction to steel making processes
 
Austempering and Martempering in Metallurgy
Austempering and Martempering in Metallurgy Austempering and Martempering in Metallurgy
Austempering and Martempering in Metallurgy
 
Ductile to brittle transition
Ductile to brittle transitionDuctile to brittle transition
Ductile to brittle transition
 

Destaque

Presentation high voltage electron microscope
Presentation high voltage electron microscopePresentation high voltage electron microscope
Presentation high voltage electron microscope
Gulfam Hussain
 
Cells and batteries
Cells and batteriesCells and batteries
Cells and batteries
Amy Gilewska
 
Mechanisms of corrosion and oxidation lecture
Mechanisms of corrosion and oxidation lectureMechanisms of corrosion and oxidation lecture
Mechanisms of corrosion and oxidation lecture
Maria Auxiliadora Silva
 

Destaque (20)

Forms of corrosion
Forms of corrosionForms of corrosion
Forms of corrosion
 
Types of corrosions
Types of corrosionsTypes of corrosions
Types of corrosions
 
Corrosion.ppt
Corrosion.pptCorrosion.ppt
Corrosion.ppt
 
Mechanism Of Dry Corrosion
Mechanism Of Dry CorrosionMechanism Of Dry Corrosion
Mechanism Of Dry Corrosion
 
corrosion presentation
corrosion presentationcorrosion presentation
corrosion presentation
 
Presentation high voltage electron microscope
Presentation high voltage electron microscopePresentation high voltage electron microscope
Presentation high voltage electron microscope
 
DLC coatings in oil and gas production
DLC coatings in oil and gas productionDLC coatings in oil and gas production
DLC coatings in oil and gas production
 
Functional surfaces for corrosion protection – current challenges and future ...
Functional surfaces for corrosion protection – current challenges and future ...Functional surfaces for corrosion protection – current challenges and future ...
Functional surfaces for corrosion protection – current challenges and future ...
 
Presentation ON EROSION CORROSION
Presentation ON EROSION CORROSIONPresentation ON EROSION CORROSION
Presentation ON EROSION CORROSION
 
Galvanic corrosion
Galvanic corrosionGalvanic corrosion
Galvanic corrosion
 
Galvanizing Methods
Galvanizing MethodsGalvanizing Methods
Galvanizing Methods
 
K to 12 smaw welding teacher's guide
K to 12 smaw welding teacher's guideK to 12 smaw welding teacher's guide
K to 12 smaw welding teacher's guide
 
Improving your SMAW welding technique
Improving your SMAW welding technique Improving your SMAW welding technique
Improving your SMAW welding technique
 
Power point presentation based on electroplating
Power point presentation based on electroplatingPower point presentation based on electroplating
Power point presentation based on electroplating
 
SMAW welding techniques
SMAW welding techniquesSMAW welding techniques
SMAW welding techniques
 
Cells and batteries
Cells and batteriesCells and batteries
Cells and batteries
 
cladding
claddingcladding
cladding
 
Production of x rays & generators
Production of x rays & generatorsProduction of x rays & generators
Production of x rays & generators
 
Mechanisms of corrosion and oxidation lecture
Mechanisms of corrosion and oxidation lectureMechanisms of corrosion and oxidation lecture
Mechanisms of corrosion and oxidation lecture
 
Eight forms of corrosion
Eight forms of corrosionEight forms of corrosion
Eight forms of corrosion
 

Semelhante a Eight forms of corrosion

Corrosion protection of metals
Corrosion protection of metalsCorrosion protection of metals
Corrosion protection of metals
Awais Chaudhary
 
Investigatory project Chemistry.docx
Investigatory project Chemistry.docxInvestigatory project Chemistry.docx
Investigatory project Chemistry.docx
Dheebannambishwar
 
It is basically slides of corrosion andr
It is basically slides of corrosion andrIt is basically slides of corrosion andr
It is basically slides of corrosion andr
AliRammaz
 
Design of a Cathodic Protection System for Corrosion Prevention of a Pipeline...
Design of a Cathodic Protection System for Corrosion Prevention of a Pipeline...Design of a Cathodic Protection System for Corrosion Prevention of a Pipeline...
Design of a Cathodic Protection System for Corrosion Prevention of a Pipeline...
Onyedikachi Martins
 
CORROSION.ppt..............,...............
CORROSION.ppt..............,...............CORROSION.ppt..............,...............
CORROSION.ppt..............,...............
PrajwalKR21
 
Investigatory project CHEMISTRY.pdf
Investigatory project CHEMISTRY.pdfInvestigatory project CHEMISTRY.pdf
Investigatory project CHEMISTRY.pdf
Dheebannambishwar
 

Semelhante a Eight forms of corrosion (20)

Rusting Of Iron
Rusting Of Iron Rusting Of Iron
Rusting Of Iron
 
Corrosion and prevention basic principles-write-up
Corrosion and prevention basic principles-write-upCorrosion and prevention basic principles-write-up
Corrosion and prevention basic principles-write-up
 
Corrosion Basics.pdf
Corrosion Basics.pdfCorrosion Basics.pdf
Corrosion Basics.pdf
 
Corrosion protection of metals
Corrosion protection of metalsCorrosion protection of metals
Corrosion protection of metals
 
Investigatory project Chemistry.docx
Investigatory project Chemistry.docxInvestigatory project Chemistry.docx
Investigatory project Chemistry.docx
 
Chemistry project
Chemistry projectChemistry project
Chemistry project
 
Tarnish & corrosion
Tarnish & corrosionTarnish & corrosion
Tarnish & corrosion
 
STUDY OF THE EFFECT OF METAL COUPLING ON THE RUSTING OF IRON
STUDY OF THE EFFECT OF METAL COUPLING ON THE RUSTING OF IRONSTUDY OF THE EFFECT OF METAL COUPLING ON THE RUSTING OF IRON
STUDY OF THE EFFECT OF METAL COUPLING ON THE RUSTING OF IRON
 
Corrosion
CorrosionCorrosion
Corrosion
 
Corrosion
CorrosionCorrosion
Corrosion
 
Corrosion.pptx
Corrosion.pptxCorrosion.pptx
Corrosion.pptx
 
It is basically slides of corrosion andr
It is basically slides of corrosion andrIt is basically slides of corrosion andr
It is basically slides of corrosion andr
 
CORROSION ENGINEERING.pptx
CORROSION ENGINEERING.pptxCORROSION ENGINEERING.pptx
CORROSION ENGINEERING.pptx
 
Design of a Cathodic Protection System for Corrosion Prevention of a Pipeline...
Design of a Cathodic Protection System for Corrosion Prevention of a Pipeline...Design of a Cathodic Protection System for Corrosion Prevention of a Pipeline...
Design of a Cathodic Protection System for Corrosion Prevention of a Pipeline...
 
Corrosion And Its Prevention (Electrochemical Interpretation)
Corrosion And Its Prevention (Electrochemical Interpretation) Corrosion And Its Prevention (Electrochemical Interpretation)
Corrosion And Its Prevention (Electrochemical Interpretation)
 
Corrosion and Its Types (Basic Chemistry - B.Tech / B.E. ))
Corrosion and Its Types (Basic Chemistry - B.Tech / B.E. ))Corrosion and Its Types (Basic Chemistry - B.Tech / B.E. ))
Corrosion and Its Types (Basic Chemistry - B.Tech / B.E. ))
 
I/II SEM BE, VTU, ENGINEERING CHEMISTRY , Module 2
I/II SEM BE, VTU, ENGINEERING CHEMISTRY , Module 2I/II SEM BE, VTU, ENGINEERING CHEMISTRY , Module 2
I/II SEM BE, VTU, ENGINEERING CHEMISTRY , Module 2
 
CORROSION.ppt..............,...............
CORROSION.ppt..............,...............CORROSION.ppt..............,...............
CORROSION.ppt..............,...............
 
Investigatory project CHEMISTRY.pdf
Investigatory project CHEMISTRY.pdfInvestigatory project CHEMISTRY.pdf
Investigatory project CHEMISTRY.pdf
 
Corrosion science by roshni pattanayak
Corrosion science  by roshni pattanayak Corrosion science  by roshni pattanayak
Corrosion science by roshni pattanayak
 

Mais de Gulfam Hussain

Mais de Gulfam Hussain (20)

Tensile, Impact and Hardness Testing of Mild Steel
Tensile, Impact and Hardness Testing of Mild SteelTensile, Impact and Hardness Testing of Mild Steel
Tensile, Impact and Hardness Testing of Mild Steel
 
Fuel cladding materials
Fuel cladding materialsFuel cladding materials
Fuel cladding materials
 
Definitions
Definitions Definitions
Definitions
 
Properties of materials / Mechanical Properties of materials
Properties of materials / Mechanical Properties of materialsProperties of materials / Mechanical Properties of materials
Properties of materials / Mechanical Properties of materials
 
Hardening (Heat treatment) Quenching
Hardening (Heat treatment)  QuenchingHardening (Heat treatment)  Quenching
Hardening (Heat treatment) Quenching
 
Extrusion
ExtrusionExtrusion
Extrusion
 
Cathode Ray Oscilloscope CRO
Cathode Ray Oscilloscope CROCathode Ray Oscilloscope CRO
Cathode Ray Oscilloscope CRO
 
Non-destructive Testing
Non-destructive TestingNon-destructive Testing
Non-destructive Testing
 
Non-traditional manufacturing processes
Non-traditional manufacturing processesNon-traditional manufacturing processes
Non-traditional manufacturing processes
 
Pakistan
PakistanPakistan
Pakistan
 
Terrorism in pakistan causes & remedies
Terrorism in pakistan causes & remediesTerrorism in pakistan causes & remedies
Terrorism in pakistan causes & remedies
 
Heat Treatment
Heat TreatmentHeat Treatment
Heat Treatment
 
Atomic Bonding
Atomic BondingAtomic Bonding
Atomic Bonding
 
Metallurgical properties of cast irons
Metallurgical properties of cast ironsMetallurgical properties of cast irons
Metallurgical properties of cast irons
 
PYROMETER
PYROMETER PYROMETER
PYROMETER
 
Muffle furnace
Muffle furnaceMuffle furnace
Muffle furnace
 
Atmospheric Corrosion
Atmospheric CorrosionAtmospheric Corrosion
Atmospheric Corrosion
 
Erosion Corrosion
Erosion Corrosion Erosion Corrosion
Erosion Corrosion
 
Optical/ Metallurgical Microscopy
Optical/ Metallurgical MicroscopyOptical/ Metallurgical Microscopy
Optical/ Metallurgical Microscopy
 
Corrosion of aluminum alloys
Corrosion of aluminum alloysCorrosion of aluminum alloys
Corrosion of aluminum alloys
 

Último

Digital Communication Essentials: DPCM, DM, and ADM .pptx
Digital Communication Essentials: DPCM, DM, and ADM .pptxDigital Communication Essentials: DPCM, DM, and ADM .pptx
Digital Communication Essentials: DPCM, DM, and ADM .pptx
pritamlangde
 
Cara Menggugurkan Sperma Yang Masuk Rahim Biyar Tidak Hamil
Cara Menggugurkan Sperma Yang Masuk Rahim Biyar Tidak HamilCara Menggugurkan Sperma Yang Masuk Rahim Biyar Tidak Hamil
Cara Menggugurkan Sperma Yang Masuk Rahim Biyar Tidak Hamil
Cara Menggugurkan Kandungan 087776558899
 
DeepFakes presentation : brief idea of DeepFakes
DeepFakes presentation : brief idea of DeepFakesDeepFakes presentation : brief idea of DeepFakes
DeepFakes presentation : brief idea of DeepFakes
MayuraD1
 
XXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXX
XXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXX
XXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXX
ssuser89054b
 
"Lesotho Leaps Forward: A Chronicle of Transformative Developments"
"Lesotho Leaps Forward: A Chronicle of Transformative Developments""Lesotho Leaps Forward: A Chronicle of Transformative Developments"
"Lesotho Leaps Forward: A Chronicle of Transformative Developments"
mphochane1998
 
Integrated Test Rig For HTFE-25 - Neometrix
Integrated Test Rig For HTFE-25 - NeometrixIntegrated Test Rig For HTFE-25 - Neometrix
Integrated Test Rig For HTFE-25 - Neometrix
Neometrix_Engineering_Pvt_Ltd
 
scipt v1.pptxcxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxx...
scipt v1.pptxcxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxx...scipt v1.pptxcxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxx...
scipt v1.pptxcxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxx...
HenryBriggs2
 

Último (20)

Digital Communication Essentials: DPCM, DM, and ADM .pptx
Digital Communication Essentials: DPCM, DM, and ADM .pptxDigital Communication Essentials: DPCM, DM, and ADM .pptx
Digital Communication Essentials: DPCM, DM, and ADM .pptx
 
Double Revolving field theory-how the rotor develops torque
Double Revolving field theory-how the rotor develops torqueDouble Revolving field theory-how the rotor develops torque
Double Revolving field theory-how the rotor develops torque
 
NO1 Top No1 Amil Baba In Azad Kashmir, Kashmir Black Magic Specialist Expert ...
NO1 Top No1 Amil Baba In Azad Kashmir, Kashmir Black Magic Specialist Expert ...NO1 Top No1 Amil Baba In Azad Kashmir, Kashmir Black Magic Specialist Expert ...
NO1 Top No1 Amil Baba In Azad Kashmir, Kashmir Black Magic Specialist Expert ...
 
DC MACHINE-Motoring and generation, Armature circuit equation
DC MACHINE-Motoring and generation, Armature circuit equationDC MACHINE-Motoring and generation, Armature circuit equation
DC MACHINE-Motoring and generation, Armature circuit equation
 
Bhubaneswar🌹Call Girls Bhubaneswar ❤Komal 9777949614 💟 Full Trusted CALL GIRL...
Bhubaneswar🌹Call Girls Bhubaneswar ❤Komal 9777949614 💟 Full Trusted CALL GIRL...Bhubaneswar🌹Call Girls Bhubaneswar ❤Komal 9777949614 💟 Full Trusted CALL GIRL...
Bhubaneswar🌹Call Girls Bhubaneswar ❤Komal 9777949614 💟 Full Trusted CALL GIRL...
 
Cara Menggugurkan Sperma Yang Masuk Rahim Biyar Tidak Hamil
Cara Menggugurkan Sperma Yang Masuk Rahim Biyar Tidak HamilCara Menggugurkan Sperma Yang Masuk Rahim Biyar Tidak Hamil
Cara Menggugurkan Sperma Yang Masuk Rahim Biyar Tidak Hamil
 
DeepFakes presentation : brief idea of DeepFakes
DeepFakes presentation : brief idea of DeepFakesDeepFakes presentation : brief idea of DeepFakes
DeepFakes presentation : brief idea of DeepFakes
 
Thermal Engineering -unit - III & IV.ppt
Thermal Engineering -unit - III & IV.pptThermal Engineering -unit - III & IV.ppt
Thermal Engineering -unit - III & IV.ppt
 
FEA Based Level 3 Assessment of Deformed Tanks with Fluid Induced Loads
FEA Based Level 3 Assessment of Deformed Tanks with Fluid Induced LoadsFEA Based Level 3 Assessment of Deformed Tanks with Fluid Induced Loads
FEA Based Level 3 Assessment of Deformed Tanks with Fluid Induced Loads
 
XXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXX
XXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXX
XXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXX
 
"Lesotho Leaps Forward: A Chronicle of Transformative Developments"
"Lesotho Leaps Forward: A Chronicle of Transformative Developments""Lesotho Leaps Forward: A Chronicle of Transformative Developments"
"Lesotho Leaps Forward: A Chronicle of Transformative Developments"
 
Thermal Engineering-R & A / C - unit - V
Thermal Engineering-R & A / C - unit - VThermal Engineering-R & A / C - unit - V
Thermal Engineering-R & A / C - unit - V
 
Integrated Test Rig For HTFE-25 - Neometrix
Integrated Test Rig For HTFE-25 - NeometrixIntegrated Test Rig For HTFE-25 - Neometrix
Integrated Test Rig For HTFE-25 - Neometrix
 
PE 459 LECTURE 2- natural gas basic concepts and properties
PE 459 LECTURE 2- natural gas basic concepts and propertiesPE 459 LECTURE 2- natural gas basic concepts and properties
PE 459 LECTURE 2- natural gas basic concepts and properties
 
scipt v1.pptxcxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxx...
scipt v1.pptxcxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxx...scipt v1.pptxcxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxx...
scipt v1.pptxcxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxxx...
 
data_management_and _data_science_cheat_sheet.pdf
data_management_and _data_science_cheat_sheet.pdfdata_management_and _data_science_cheat_sheet.pdf
data_management_and _data_science_cheat_sheet.pdf
 
Generative AI or GenAI technology based PPT
Generative AI or GenAI technology based PPTGenerative AI or GenAI technology based PPT
Generative AI or GenAI technology based PPT
 
457503602-5-Gas-Well-Testing-and-Analysis-pptx.pptx
457503602-5-Gas-Well-Testing-and-Analysis-pptx.pptx457503602-5-Gas-Well-Testing-and-Analysis-pptx.pptx
457503602-5-Gas-Well-Testing-and-Analysis-pptx.pptx
 
HAND TOOLS USED AT ELECTRONICS WORK PRESENTED BY KOUSTAV SARKAR
HAND TOOLS USED AT ELECTRONICS WORK PRESENTED BY KOUSTAV SARKARHAND TOOLS USED AT ELECTRONICS WORK PRESENTED BY KOUSTAV SARKAR
HAND TOOLS USED AT ELECTRONICS WORK PRESENTED BY KOUSTAV SARKAR
 
Hostel management system project report..pdf
Hostel management system project report..pdfHostel management system project report..pdf
Hostel management system project report..pdf
 

Eight forms of corrosion

  • 1. The 8 Forms of Corrosion M.E. 464 Brett A. Anderson December 20, 2001
  • 2. Corrosion is a costly and potentially life threatening problem in any industry. Wherever there is metal the potential for a corrosive reaction exists. It is a natural part of nature, there is no escaping it. That doesn’t mean that we are doomed though. Through a careful analysis of the process and the design we can mitigate most of the costs of corrosion, both actual and potential, before the first pipe is in place. The science of corrosion engineering is viewed by many as magic, or art, but once the basics of how a corrosion cell works and a little understanding of chemistry almost anyone can learn to decipher the clues to the causes of a corrosion problem. Most corrosion problems encountered fall into five basic categories: • Uniform or general corrosion: this is the most common form of corrosion encountered. • Localized corrosion: as the name implies this form of corrosion occurs in discreet areas on the surface of the metal. • Metallurgically induced corrosion: this form of corrosion attacks the metal’s physical and chemical makeup. • Mechanically assisted corrosion: the physical parameters of the system play an important part in this form of corrosion. • Stress corrosion cracking: this form of corrosion results in cracks in the metal that are induced by both stresses and corrosive elements. With this information we can hopefully reduce the costs of replacing expensive assets before they have fully depreciated, but our ultimate goal is to reduce the chances of a catastrophic failure or loss of life due to a corroded system.
  • 3. Thermodynamic and Electrochemical Processes The corrosion process of metals is a natural result of the inherent tendency to revert to a more stable compound, such as an oxide. Metal ore that is mined must be refined and then alloyed for use. Energy is required to refine these ores into useable metals. Entropy, a thermodynamic property, drives these metals to corrode. “Every system which is left to itself will, on the average, change toward a condition of maximum probability.” (G. N. Lewis) Energy is required to keep these metals in the refined state and when left alone they will, over time, revert back to the more stable compounds in which they occur naturally. An example of this is iron. Hematite is the principle ore of iron. Hematite is a form of iron oxide, its chemical composition is FE2O3. Processed iron ore, coke, and limestone are added to the top of a blast furnace (Figure 1-1).1 The coke is the source of the chemical energy in the blast furnace. When it is burnt by the hot air it releases both heat energy and the main reducing agent, CO. 2C + O2 ∆H 2CO ∆H = -394 kJ/mol The limestone is decomposed by the heat into calcium oxide, CaO, and additional carbon monoxide. 2CaCO3 ∆H 2CaO + 2CO + O2 The main chemical reaction takes place, and the calcium oxide combines with the impurities in the ore to form slag. Fe2O3 + 3CO ∆H 3CO2 + 2Fe The refined iron then runs down and out of the blast furnace to form pig iron. The pig iron is then combined with other alloys to get different kinds of steels. 1 U.S. Department of Energy's Office of Fossil Energy website (December 14, 2001). Figure 1-1. The blast furnace is used to turn iron ore into pig iron for the steel making process.
  • 4. At this point, the second law of thermodynamics and free energy come into play. The second law of thermodynamics quite simply states: “The stable, equilibrium state of a system is the state of minimum free energy.”2 Iron in the processed form, Fe, has a greater amount of free energy than iron oxide. That energy was added when the ore was heated in the blast furnace. The system, in this case the processed iron, will always be headed towards its most stable state, which is the state of minimum free energy. When moisture and oxygen are present the iron will undergo a chemical reaction to reduce the amount of free energy available. This redox, reduction oxidation, reaction produces hydrated iron oxide: 4Fe+2 (aq) + O2(g) + [(4 + 2x)H2O](l) [2Fe2O3 · xH2O](s) + 8H+ (aq) The resulting iron oxide, Fe2O3, is one of the most stable states for iron to be found in. This simple example of an electrochemical reaction demonstrates one of the most important principles of metallic corrosion: the rate of oxidation equals the rate of reduction.3 It is important to note that when alloys are corroded more than one oxidation and one reduction reaction can occur. Another way of looking at the corrosion process is as a series of anodic and cathodic reactions. In this situation four elements are necessary for corrosion to occur: • An anode. • A cathode. • An electrolyte (water) • A metallic path for electron flow. When all four of these elements are present a corrosion cell is formed. It is important to remember that the anodic and cathodic reactions do not have to occur at the same spot on the material. As long as an electrolyte and a metallic path exist, these half- cells can exist and corrosion will occur. Figure 1-2 is an example of the corrosion cell with the four elements labeled.4 2 Davis, Neil T. (2001) page 37. 3 Fontana, Mars G. (1986) page 15. 4 Allen, Thomas O., Roberts, Alan P. (1993) page 10-1, 10-2. Figure 1-2. Corrosion cell diagram depicting the current flow from the corrosion pit.
  • 5. The same redox reactions that occurred in the afore mentioned example are occurring in the corrosion cell. The oxidation reaction takes place at the anode, and the reduction reaction takes place at the cathode. It is this series of oxidation and reduction reactions that make up the electrochemistry of the corrosion process. It is important to note that there is a flow of electrons from one half-cell to the other during the corrosion process. The electric current flows from the anodes to the cathodes of the reaction through the electrolyte. The flow of electric current in the corrosion cell per unit area is referred to as the Corrosion Current Density (icorr). As each oxidation reaction occurs a transfer of electrons to the electrolyte occurs. Since icorr is a measure of current flow per unit area per unit time it can be seen that icorr can be related to units of metal loss per unit time. Corrosion rates are generally expressed in mils per year of metal thickness reduction (MPY), so icorr is a good representative of the corrosion rate in the cell.5 Armed with this information it is possible to slow down or even prevent the corrosion from occurring by increasing the resistance in the electrochemical corrosion circuit. Adding chemical inhibitors and coatings to the materials to reduce the current flow will help to increase the circuit resistance. The free energy available in the metal and in the electrolyte creates a potential at the anode and at the cathode. It is the difference in potential between these two sites that causes the electron flow. Most corrosion reactions are considered wet and occur in the presence of a liquid. Marcel Pourbiax, a well-known Belgian scientist, developed a diagram which relates the stability of a metal in a given pH environment in 1938. By plotting the potential of a metal and the pH of the environment it is possible to determine if the metal is in a region where the possibility of corrosion is high, the possibility for corrosion is non-existent, or the possibility exists but there is a tendency for the development of a protective film. Figure 1-3 is the Pourbiax diagram for an iron-water system at 25 degrees Celsius.6 The gray zone represents the area where the base metal, iron, is stable. This is the region where the possibility of corrosion is non-existent. The orange zone is where rust, the non-protective form of corroded iron, is expected. The blue zone is where the most stable iron species, Fe(OH)2, is encountered. This species is called blue rust and is fairly rare and highly soluble. The white areas are where corrosion is most probable. 5 Rohrback Casaco Systems website (December 14, 2001) page 3. 6 Corrosion Doctors website (December 13, 2001). Figure 1-3. Pourbiax diagram for an iron-water system at 25û C.
  • 6. These Pourbiax diagrams are time consuming to create and a new diagram must be created for each metal or alloy that is being used and the environment it is in. There are software programs available that can produce these diagrams for the student of corrosion processes.7 It is not enough to determine if the possibility for corrosion exists, a corrosion rate must also be determined. It is entirely possible for the probability of corrosion to be high and resultant corrosion rates to be very low. In these cases the corrosion might not be a problem. Corrosion rates are determined through polarization curves. Polarization curves are produced through the application of a current to the metal surface. If the potential of the metal surface is polarized by the current in a positive sense it is referred to as being anodically polarized; a negative sense signifies that it is cathodically polarized. The degree of polarization is a measure of how the rates of the anodic and cathodic reactions are hindered by various environmental and surface process factors. The environmental factors (the concentrations of metal ions, dissolved oxygen in the solution, etc.) are referred to as the concentration polarization. The surface process factors (film formation, adsorption, etc.) are referred to as the activation polarization. The polarization curve is a graph of the variation of the potential as a function of the current, which allows the effects of the concentration and activation processes on the rate at which the anodic or cathodic reactions can give or receive electrons to be determined. This allows for a rate determination for the reactions that are involved in the corrosion process, in effect a corrosion rate.8 7 Corrosion Doctors website (December 13, 2001). 8 Encyclopedia of Electrochemistry website (December 13, 2001) page 5. Figure 1-4. General Polarization curve for a material with both anodic and cathodic polarization curves.
  • 7. The polarization curve above shows the polarization curves for both anodic and cathodic reactions. The potential, E, is plotted as a function of the logarithm of icorr. Ecorr, the corrosion potential, is determined by the intersection of the extrapolation of the linear portions of the anodic and cathodic polarization curves. The value of the current at the intersection is the rate of corrosion expressed in current density, icorr. From this polarization curve the Evans diagram can be extrapolated. Evans diagrams are useful in determining if the anodic, cathodic, or both reactions control the rate of the corrosion. Figure 1-5 shows the three types of Evans diagrams that can be extrapolated from the polarization curve, (a) shows that the rate is controlled by the anodic reaction, (b) is controlled by the cathodic reaction, and (c) is controlled by a combination of both reactions. This information is used by corrosion engineers to allow the evaluation of the effects of measurable factors, which can be controlled, on the rates of corrosion.9 Another determining factor in the corrosion rate is the phenomenon of passivity and passive films. Passivity generally refers to materials that form insoluble films, which inhibit the anodic reactions and cause a polarization of the anode.10 These films can markedly reduce the rate of corrosion as long as they are not breached. These films can experience breakdowns from both electrochemical reactions and mechanical mechanisms. Those discrete sites where a breach in the film occurs can experience an accelerated rate of corrosion. One of the major causes of the breaching of the passive films is the chloride ion, which is readily available in nature. 9 Encyclopedia of Electrochemistry website (December 13, 2001) page 6. 10 Atkinson, J.T.N., Van Droffelaar, H. (1995) page 54. Figure 1-5. Evans diagram extrapolated from the polarization curve (a) shows that the rate is controlled by the anodic reaction, (b) is controlled by the cathodic reaction, and (c) is controlled by a combination of both reactions.
  • 8. An interesting process that some alloys undergo is repassivation. This process is very effective for combating localized corrosion. These alloys form a passive film that resists the breakdown process in a fairly effective manor, and are capable of repassivating at a rate high enough that once a breach has occurred the exposure to the corrosive environment is reduced to a minimum.11 Forms of Corrosion From the engineers standpoint the forms that corrosion takes can generally be identified by a visual examination. It is usually possible to determine a probable mechanism for the corrosion by corresponding the corrosion in question to one or more of general forms. • Uniform or General corrosion: a regular loss of metal from the surface cases a uniform thinning. • Localized corrosion: the majority of metal loss is experienced in discrete areas. • Metallurgically Induced corrosion • Mechanically Assisted corrosion: physical environmental factors play a significant role in metal loss. • Stress corrosion: generally cracking that is induced by environmental factors. These five basic types of corrosion can be broken down into eight visually identifiable forms, which are significantly different from one another. This allows an engineer to examine a specimen and make a reasonable assumption on the general cause of the corrosion and possible corrective measures that can be taken. General Corrosion General corrosion, or uniform attack, is the most common form of corrosion. General corrosion occurs uniformly over the entire surface that is exposed. The metal gets thinner evenly over the entire surface, leading this form of corrosion to account for the largest tonnage of metal loss. This form of corrosion is generally the cheapest form of corrosion to deal with in industry. It is fairly consistent and rates can quickly be found by exposing a sample to the environment. Making the material thicker than necessary to accommodate the corrosion throughout the life of the product, or applying a coating to the surface, such as paint, are the standard methods of prevention for this form of corrosion. 11 Encyclopedia of Electrochemistry website (December 13, 2001) page 6. Photo 2-1. Depicts general, or uniform, corrosion on a steel fitting.
  • 9.
  • 10. Galvanic Corrosion Galvanic, or two-metal, corrosion occurs because of the potential difference that exists between two dissimilar metals. When these two metals can be connected electrically, either through direct contact or an electrolyte, the difference in potential causes a flow of electrons, or current, between them. The further apart on the Galvanic Scale (figure 2-1) that these two metals are increases the amount of corrosion experienced by anodic member of the galvanic couple. The ensuing corrosion reaction is a perfect example of the corrosion cell in figure 1-2. The corrosion resistant, or noble, metal becomes the cathode and experiences very little, if any metal loss. While the less corrosion resistant metal becomes the anode. Figure 2-1. The Galvanic Scale. Photo 2-5. Galvanic corrosion of a bolt. Photo 2-6. Light galvanic corrosion around a bolt on a pump housing.
  • 11. Proper material selection can eliminate most of the problems associated with galvanic corrosion. Combinations of metals and alloys used together should not be widely separated on the galvanic scale. Dissimilar metal crevices, such as threaded connections, should be avoided, and fasteners of the same material or a more noble material should be used.12 Crevice Corrosion Crevice corrosion is an intensive, localized form of corrosion. It generally occurs in cracks, holes, crevices, lap joints, under gaskets, rivet and bolt heads, and anywhere else that small amounts of solution can lay stagnate. Crevice corrosion begins with the typical corrosion cell (figure 1-2), an oxygen concentration cell. As the oxygen is depleted the growth of the corrosion cell is driven by the accumulation of acidic hydrolyzed salts in the crevice area. 12 Dillon, C.P. (1982) page 47. Photo 2-7. Galvanic corrosion at the threaded connection between a brass fitting and a steel backwash line for a water softener. Photo 2-8. Corrosion of a brass fitting due to the galvanic couple created with the copper pipe. Photo 2-9. Failure due to crevice corrosion in the threaded area of a pipe.
  • 12. Proper material selection and design features that limit the number of crevices and allow for drainage are the most effective way of mitigating the effects of crevice corrosion. Photo 2-10. Excellent example of crevice corrosion on several fronts. Notice the extensive corrosion between the flange faces, and the corrosion of the bolts that held the flange together. Photo 2-11. Crevice corrosion is very common in tube and shell heat exchangers. The main areas of concern are where the tubes enter the tube sheets and where they go through the baffles. Photo courtesy Tim Milanowski.
  • 13. Pitting Pitting is a troublesome form of corrosion. It can cause a failure with very little metal loss. Pitting is an extremely localized form of attack that often causes rapid penetration of the wall thickness.13 The holes that pitting causes can be very small or quite large in diameter. The fact that failure can occur with very little metal loss and with just one little area affected is what makes this form of corrosion so difficult to detect and prevent. 13 Dillon, C.P. (1982) page 19. Photo 2-12. Large pit that occurred in an oily water line, this pit had penetrated about 90% of the way through the wall. Photo 2-13. This is an oily water line, and the glycol tracing that was welded to it, that experienced failure due to pitting. Notice that the pitting occurs on the bottom half of the pipe. Pits usually grow in the direction of gravity. The largest pits and the failure occurred in the heat-affected zone where the glycol heat trace was welded to the pipe.
  • 14. Photos 2-14, 2-15, and 2-16 show how varied small pits can be. In order to detect that there is a problem you would have to use UT, and be lucky enough to be right on top of the pit. Intergranular Corrosion Intergranular corrosion is the corrosion of the edges of the individual grains that make up the metal. The preferential attack along the grain boundaries can lead to a decrease in effective cross section of material and eventual mechanical failure.14 Metals experiencing intergranular corrosion that should otherwise exhibit excellent corrosion resistant tendencies have been sensitized. Sensitizing usually occurs through damaging thermal exposures, such as welding. Material selection, heat-treating, quenching, and proper welding techniques are effective methods for avoiding intergranular corrosion. 14 Dillon, C.P. (1982) page 89. Photo 2-14 (upper left). Hole in oily water line caused by pitting. Photo 2-15 (upper right). Wormhole pit in a 1-inch diameter steel water pipe. Photo 2-16 (left). Failure caused by a small pit. Photo 2-17. This is the heat-affected zone from photo 2-13. This is a case of weld decay in the heat-affected zone.
  • 15. Selective Leaching Selective leaching, or dealloying, is the removal of one element from an alloy through a corrosion process. The most common form of dealloying is the removal of zinc from brass alloys. Common yellow brass is 30% zinc and 70% copper. The brass turns a red or copper color that contrasts with the original yellow brass, or zinc oxide builds up on the outside of the brass piece. Photo 2-18. Heat-affected zone of a circumferential weld is very distinct in this photo. Photo 2-21 and Photo 2-22. Dezincification of a brass valve. Photo 2-19 and 2-20. Carburization, a special case of intergranular corrosion. This steel hook has undergone carburization at high temperatures.
  • 16. Erosion Corrosion Erosion corrosion is the accelerated increase in deterioration of a metal due to the velocity of the fluid. The fluid does not have to contain any abrasive particles, but the metal will be worn away faster if there are abrasives present. Photo 2-23. The velocity effects of the shell side fluid in the tube and shell exchanger are quite obvious. Photo courtesy Tim Milanowski. Photo 2-24. Hole in the HAZ. This failure was caused by erosion corrosion. Notice the shape of the pits, they are deeper on the downstream side (above the weld line). Here is a good case of two forms of corrosion working together. The failure is actually in the heat-affected zone of the weld, but it is obvious that erosion played the bigger part in creating the hole itself. This is from a section of piping just downstream of a flow meter. In order for the flow meter to work properly the diameter of the pipe was reduced several feet upstream of the meter. This reduction in diameter increased the velocity through the section of pipe. Photo courtesy Tim Milanowski.
  • 17. Photo 2-25. This photo illustrates unique patterns that occur in some of the erosion corrosion cases. Photo 2-26. Severe erosion corrosion around a nozzle in a tube and shell heat exchanger. Photo courtesy Tim Milanowski. Photo 2-27. Severe erosion corrosion due to impingement in a tube and shell heat exchanger. Photo courtesy Tim Milanowski.
  • 18. Stress Corrosion Cracking Stress corrosion cracking (SCC) is the cracking from a combined presence of tensile stresses and a corrosive medium. The tensile stresses can come from applied stresses or residual stresses. Residual stresses are introduced into a material through forming, welding, machining, heat treatments, and grinding. The metal remains unattacked over its surface, while fine cracks progress through it. Summary Through a visual examination it is often possible to classify a corrosion problem by the forms of corrosion that are present. The type of corrosion present tells a lot about the corrosion mechanisms involved and possible methods to control or alleviate the Photo 2-28. This is part of a sump float that exhibits signs of chloride induced stress corrosion cracking. The cracks are at right angles to the setscrew, which is where the ring would experience the greatest stresses. Photo 2-29. More Chloride induced stress corrosion cracking. These two pieces are from the same sump as photo 2-28.
  • 19. corrosion problem. Corrosion can usually be placed in to one or more of the following visual forms: • General or Uniform Corrosion. • Galvanic Corrosion. • Crevice Corrosion. • Pitting. • Intergranular Corrosion. • Selective Leeching. • Erosion Corrosion. • Stress Corrosion Cracking. Through a careful analysis of the problem a method to avoid any similar problems in the future can be found. The most important part of any design from the corrosion standpoint is: Are the materials chosen the right materials for the job, and will they work together? The Last Exchange. Photo by Tim Milanowski.
  • 20. References: About.com Chemistry website (December 4, 2001) http://chemengineer.about.com/cs/corrosion1/index.htm. Allen, Thomas O., Roberts, Alan P. (1993) Productions Operations Volume 2 (Oil & Gas Consultants International, Inc.: Tulsa, Oklahoma). Alyeska Pipeline Company website (December 12, 2001) http://www.alyeska- pipe.com/pipelinefacts.html. Atkinson, J.T.N., Van Droffelaar, H. (1995) Corrosion and Its Control (NACE International: Houston, Texas). Boteler, D.H., Seager, W.H., Johanson, C., and Harde, C. (1999) Cold Climate Corrosion Special Topics: Telluric Current Effects on Long and Short Pipelines (NACE International: New York, New York) pp 67-79. Corrosion Doctors website (December 13, 2001) http://www.corrosion-doctors.org. Corrosion Research Center website (December 1, 2001) http://www3.cems.umn.edu/research/crc/. Corrosion Source website (December 4, 2001) http://www.corrosionsource.com. Corrosion Technology Testbed website (December 11, 2001) http://corrosion.kcs.nasa.gov/html/crevcor.htm. Davis, Neil T. (2001) Permafrost A Guide To Frozen Ground in Transition (University of Alaska Press). Dillon, C.P. (1982) Forms of Corrosion Recognition and Prevention (NACE International: Houston, Texas). Encyclopedia of Electrochemistry website (December 13, 2001) http://electrochem.cwru.edu/ed/encycl/. Fontana, Mars G. (1986) Corrosion Engineering (McGraw-Hill, Inc: New York, New York). King, R.J., White, W.E. (1999) Cold Climate Corrosion Special Topics: Thermodynamic Consideration Relevant to Corrosion of Pipeline Steels in Permafrost (NACE International: New York, New York) pp 37-66. Korb, Lawrence J., Olson, David L. (1987) Metals Handbook Ninth Edition, Volume 13 Corrosion (ASM International: Houston, Texas).
  • 21. Milanowski, Tim (December 2001) Inspection Coordinator for Williams Alaska Petroleum, North Pole, Alaska. Minnesota Power Electric website (December 12, 2001) http://www.mpelectric.com/storms/elctrjet.htm. Moniz, B.J. (1994) Metallurgy (American Technical Publishers, Inc.: Homewood, Illinois). Ryan’s Crevice Corrosion Page (December 10, 2001) http://www.personal.psu.edu/users/r/c/rcw134/crevice.html. Rohrback Casasco Systems website (December 14, 2001) http://www.corrpro.com/rcs/. Southwest Research Institute website (December 13, 2001) http://www.swri.org/3pubs/ttoday/fall96/pipe.htm. The Hendrix Group website (December 4, 2001) http://www.hghouston.com/tidbits.html. U.S. Department of Energy’s Office of Fossil Energy website (December 10, 2001) http://www.lanl.gov/projects/cctc/factsheets/bstel/blastfgrandemo.html.