Chapter 11
Phase
TransformationsFe3C (cementite)- orthorhombic
Martensite - BCT
Austenite - FCC
Ferrite - BCC
Phase Transformations
• Transformation rate
• Kinetics of Phase Transformation
–Nucleation: homogeneous, heterogeneous
–Free Energy, Growth
• Isothermal Transformations (TTT diagrams)
• Pearlite, Martensite, Spheroidite, Bainite
• Continuous Cooling
• Mechanical Behavior
• Precipitation Hardening
Phase Transformations

Phase transformations – change in the
number or character of phases.

Simple diffusion-dependent

No change in # of phases

No change in composition

Example: solidification of a pure metal, allotropic transformation,
recrystallization, grain growth

More complicated diffusion-dependent

Change in # of phases

Change in composition

Example: eutectoid reaction

Diffusionless

Example: metastable phase - martensite
Phase Transformations

Most phase transformations begin with the formation of
numerous small particles of the new phase that increase in
size until the transformation is complete.
• Nucleation is the process whereby nuclei (seeds) act as
templates for crystal growth.
• Homogeneous nucleation - nuclei form uniformly throughout
the parent phase; requires considerable supercooling
(typically 80-300°C).
• Heterogeneous nucleation - form at structural
inhomogeneities (container surfaces, impurities, grain
boundaries, dislocations) in liquid phase much easier since
stable “nucleating surface” is already present; requires
slight supercooling (0.1-10ºC).
Supercooling

During the cooling of a liquid, solidification
(nucleation) will begin only after the temperature
has been lowered below the equilibrium
solidification (or melting) temperature Tm. This
phenomenon is termed supercooling (or
undercooling.

The driving force to nucleate increases as ∆T
increases

Small supercooling  slow nucleation rate - few
nuclei - large crystals

Large supercooling  rapid nucleation rate -
many nuclei - small crystals
Nucleation of a spherical solid particle in a liquid
Liquid

The change in free energy ∆G (a function of the
internal energy and enthalpy of the system) must
be negative for a transformation to occur.

Assume that nuclei of the solid phase form in the
interior of the liquid as atoms cluster together-
similar to the packing in the solid phase.

Also, each nucleus is spherical and has a radius r.

Free energy changes as a result of a
transformation: 1) the difference between the solid
and liquid phases (volume free energy, ∆GV); and
2) the solid-liquid phase boundary (surface free
energy, ∆GS).

Transforming one phase into another takes time.
∆G = ∆GS + ∆GV
Fe
γ
(Austenite)
Eutectoid
transformation
C FCC
Fe3C
(cementite)
α
(ferrite)
+
(BCC)
r* = critical nucleus: for r < r* nuclei shrink; for r >r* nuclei grow (to reduce energy)
Homogeneous Nucleation & Energy Effects
∆GT = Total Free Energy
= ∆GS + ∆GV
Surface Free Energy- destabilizes
the nuclei (it takes energy to make
an interface)
γπ=∆ 2
4 rGS
γ = surface tension
Volume (Bulk) Free Energy –
stabilizes the nuclei (releases energy)
υ∆π=∆ GrGV
3
3
4
volumeunit
energyfreevolume
=∆ υG
Solidification
TH
T
r
f
m
∆∆
γ−
=
2
*
Note: ∆Hf and γ are weakly dependent on ∆T
∴ r* decreases as ∆T increases
For typical ∆T r* ~ 10 nm
∆Hf = latent heat of solidification (fusion)
Tm = melting temperature
γ = surface free energy
∆T = Tm - T = supercooling
r* = critical radius
Transformations & Undercooling
• For transformation to occur,
must cool to below 727°C
• Eutectoid transformation (Fe-Fe3C system): γ ⇒ α + Fe3C
0.76 wt% C
0.022 wt% C
6.7 wt% C
Fe3C(cementite)
1600
1400
1200
1000
800
600
400
0 1 2 3 4 5 6 6.7
L
γ
(austenite)
γ+L
γ +Fe3C
α +Fe3C
L+Fe3C
δ
(Fe) C, wt% C
1148°C
T(°C)
α
ferrite
727°C
Eutectoid:
Equil. Cooling: Ttransf. = 727ºC
∆T
Undercooling by Ttransf. < 727°C
0.76
0.022
2
• Fraction transformed depends on time.
fraction
transformed time
y = 1− e
−ktn
Avrami Eqn.
• Transformation rate depends on T.
1 10 102 1040
50
100
135°C
119°C113°C102°C
88°C
43°C
y (%)
log (t) min
Ex: recrystallization of Cu
r =
1
t
0.5
= Ae
−Q /RT
activation energy
• r often small: equil not possible
y
log (t)
Fixed
T
0
0.5
1
t0.5
FRACTION OF TRANSFORMATION
Generation of Isothermal Transformation Diagrams
• The Fe-Fe3C system, for Co = 0.76 wt% C
• A transformation temperature of 675°C.
100
50
0
1 102 104
T = 675°C
%transformed
time (s)
400
500
600
700
1 10 102 103 104 105
0%pearlite
100%
50%
Austenite (stable)
TE (727°C)Austenite
(unstable)
Pearlite
T(°C)
time (s)
isothermal transformation at 675°C
Consider:
Coarse pearlite  formed at higher temperatures – relatively soft
Fine pearlite  formed at lower temperatures – relatively hard
• Transformation of austenite to pearlite:
γα
α
α
α
α
α
pearlite
growth
direction
Austenite (γ)
grain
boundary
cementite (Fe3C)
Ferrite (α)
γ
• For this transformation,
rate increases with ( ∆T)
[Teutectoid – T ].
675°C
(∆T smaller)
0
50
%pearlite
600°C
(∆T larger)
650°C
100
Diffusion of C
during transformation
α
α
γ
γ
α
Carbon
diffusion
Eutectoid Transformation Rate ~ ∆T
5
• Reaction rate is a result of nucleation and growth of crystals.
• Examples:
% Pearlite
0
50
100
Nucleation
regime
Growth
regime
log (time)t50
Nucleation rate increases w/ ∆T
Growth rate increases w/ T
Nucleation rate high
T just below TE T moderately below TE T way below TE
Nucleation rate low
Growth rate high
γ γ γ
pearlite
colony
Nucleation rate med .
Growth rate med. Growth rate low
Nucleation and Growth
Isothermal Transformation Diagrams
2 solid curves are plotted:
 one represents the time
required at each
temperature for the start of
the transformation;
 the other is for
transformation completion.
 The dashed curve
corresponds to 50%
completion.
The austenite to pearlite
transformation will occur
only if the alloy is
supercooled to below the
eutectoid temperature
(727˚C).
Time for process to complete
depends on the
temperature.
• Eutectoid iron-carbon alloy; composition, Co = 0.76 wt% C
• Begin at T > 727˚C
• Rapidly cool to 625˚C and hold isothermally.
Isothermal Transformation Diagram
Austenite-to-Pearlite
Transformations Involving
Noneutectoid Compositions
Hypereutectoid composition – proeutectoid cementite
Consider C0 = 1.13 wt% C
Fe3C(cementite)
1600
1400
1200
1000
800
600
400
0 1 2 3 4 5 6 6.7
L
γ
(austenite)
γ+L
γ +Fe3C
α+Fe3C
L+Fe3C
δ
(Fe)
C, wt%C
T(°C)
727°C
∆T
0.76
0.022
1.13
Strength
Ductility
Martensite
T Martensite
bainite
fine pearlite
coarse pearlite
spheroidite
General Trends
Possible Transformations
Coarse pearlite (high diffusion rate) and (b) fine pearlite
- Smaller ∆T:
colonies are
larger
- Larger ∆T:
colonies are
smaller
10 103
105
time (s)
10-1
400
600
800
T(°C)
Austenite (stable)
200
P
B
TE
0%
100%
50%
A
A
Bainite: Non-Equil Transformation Products
 elongated Fe3C particles in α-ferrite matrix
 diffusion controlled
 α lathes (strips) with long rods of Fe3C
100% bainite
100% pearlite
Martensite
Cementite
Ferrite
Bainite Microstructure
• Bainite consists of acicular
(needle-like) ferrite with very
small cementite particles
dispersed throughout.
• The carbon content is
typically greater than 0.1%.
• Bainite transforms to iron and
cementite with sufficient time
and temperature (considered
semi-stable below 150°C).
10
 Fe3C particles within an α-ferrite matrix
 diffusion dependent
 heat bainite or pearlite at temperature just below eutectoid for long times
 driving force – reduction of α-ferrite/Fe3C interfacial area
Spheroidite: Nonequilibrium Transformation
10 103 105time (s)10-1
400
600
800
T(°C)
Austenite (stable)
200
P
B
TE
0%
100%
50%
A
A
Spheroidite
100% spheroidite
100% spheroidite
Pearlitic Steel partially transformed to Spheroidite
 single phase
 body centered tetragonal (BCT) crystal structure
 BCT if C0 > 0.15 wt% C
 Diffusionless transformation
 BCT  few slip planes  hard, brittle
 % transformation depends only on T of rapid cooling
Martensite Formation
• Isothermal Transformation Diagram
10 10
3
10
5
time (s)10
-1
400
600
800
T(°C)
Austenite (stable)
200
P
B
TE
0%
100%50%
A
A
M + A
M + A
M + A
0%
50%
90%
Martensite needles
Austenite
An micrograph of austenite that was polished flat and then
allowed to transform into martensite.
The different colors indicate the displacements caused when
martensite forms.
Isothermal Transformation Diagram
Iron-carbon alloy
with eutectoid
composition.

A: Austenite

P: Pearlite

B: Bainite

M: Martensite

Other elements (Cr, Ni, Mo, Si and
W) may cause significant changes
in the positions and shapes of the
TTT curves:

Change transition temperature;

Shift the nose of the austenite-to-
pearlite transformation to longer
times;

Shift the pearlite and bainite noses
to longer times (decrease critical
cooling rate);

Form a separate bainite nose;
Effect of Adding
Other Elements
4340 Steel
plain
carbon
steel
nose

Plain carbon steel: primary
alloying element is carbon.
Example 11.2:
 Iron-carbon alloy with
eutectoid composition.
 Specify the nature of the
final microstructure (%
bainite, martensite, pearlite
etc) for the alloy that is
subjected to the following
time–temperature
treatments:
 Alloy begins at 760˚C and
has been held long enough
to achieve a complete and
homogeneous austenitic
structure.
Treatment (a)
 Rapidly cool to 350 ˚C
 Hold for 104
seconds
 Quench to room temperature
Bainite,
100%
Martensite,
100%
Example 11.2:
 Iron-carbon alloy with
eutectoid composition.
 Specify the nature of the
final microstructure (%
bainite, martensite, pearlite
etc) for the alloy that is
subjected to the following
time–temperature
treatments:
 Alloy begins at 760˚C and
has been held long enough
to achieve a complete and
homogeneous austenitic
structure.
Treatment (b)
 Rapidly cool to 250 ˚C
 Hold for 100 seconds
 Quench to room temperature
Austenite,
100%
Bainite, 50%
Example 11.2:
 Iron-carbon alloy with
eutectoid composition.
 Specify the nature of the
final microstructure (%
bainite, martensite, pearlite
etc) for the alloy that is
subjected to the following
time–temperature
treatments:
 Alloy begins at 760˚C and
has been held long enough
to achieve a complete and
homogeneous austenitic
structure.
Treatment (c)
 Rapidly cool to 650˚C
 Hold for 20 seconds
 Rapidly cool to 400˚C
 Hold for 103
seconds
 Quench to room temperature
Austenite,
100%
Almost 50% Pearlite,
50% Austenite
Final:
50% Bainite,
50% Pearlite
Continuous Cooling
Transformation Diagrams
 Isothermal heat treatments are
not the most practical due to
rapidly cooling and constant
maintenance at an elevated
temperature.
 Most heat treatments for steels
involve the continuous cooling
of a specimen to room
temperature.
 TTT diagram (dotted curve) is
modified for a CCT diagram
(solid curve).
 For continuous cooling, the time
required for a reaction to begin
and end is delayed.
 The isothermal curves are
shifted to longer times and
lower temperatures.
 Moderately rapid and slow
cooling curves are
superimposed on a continuous
cooling transformation
diagram of a eutectoid iron-
carbon alloy.

The transformation starts after
a time period corresponding to
the intersection of the cooling
curve with the beginning
reaction curve and ends upon
crossing the completion
transformation curve.

Normally bainite does not form
when an alloy is continuously
cooled to room temperature;
austenite transforms to
pearlite before bainite has
become possible.

The austenite-pearlite region
(A---B) terminates just below
the nose. Continued cooling
(below Mstart) of austenite will
form martensite.

For continuous cooling of a
steel alloy there exists a
critical quenching rate that
represents the minimum rate
of quenching that will
produce a totally martensitic
structure.

This curve will just miss the
nose where pearlite
transformation begins

Continuous cooling
diagram for a 4340 steel
alloy and several cooling
curves superimposed.

This demonstrates the
dependence of the final
microstructure on the
transformations that occur
during cooling.

Alloying elements used to
modify the critical cooling
rate for martensite are
chromium, nickel,
molybdenum,
manganese, silicon and
tungsten.
Mechanical Properties
• Hardness
• Brinell, Rockwell
• Yield Strength
• Tensile Strength
• Ductility
• % Elongation
• Effect of Carbon Content
Mechanical Properties: Influence of Carbon Content
C0 > 0.76 wt% C
Hypereutectoid
Pearlite (med)
Cementite
(hard)
C0 < 0.76 wt% C
Hypoeutectoid
Pearlite (med)
ferrite (soft)
Mechanical Properties: Fe-C System
 Tempered martensite is less brittle than martensite; tempered at 594 °C.
 Tempering reduces internal stresses caused by quenching.
 The small particles are cementite; the matrix is α-ferrite. US Steel Corp.
Tempered Martensite
4340 steel
Hardness as a function of carbon
concentration for steels
Hardness versus tempering time for a water-quenched eutectoid plain carbon steel (1080);
room temperature.
Rockwell C and Brinell Hardness
Precipitation Hardening
• The strength and hardness of some metal
alloys may be improved by the formation of
extremely small, uniformly dispersed particles
(precipitates) of a second phase within the
original phase matrix.
• Other alloys that can be precipitation
hardened or age hardened:
 Copper-beryllium (Cu-Be)
 Copper-tin (Cu-Sn)
 Magnesium-aluminum (Mg-Al)
 Aluminum-copper (Al-Cu)
 High-strength aluminum alloys
Criteria:

Maximum solubility of 1 component
in the other (M);

Solubility limit that rapidly
decreases with decrease in
temperature (M→N).
Process:

Solution Heat Treatment – first
heat treatment where all solute
atoms are dissolved to form a
single-phase solid solution.
Heat to T0 and dissolve B phase.
Rapidly quench to T1

Nonequilibrium state (α phase solid
solution supersaturated with B
atoms; alloy is soft, weak-no ppts).
Phase Diagram for Precipitation Hardened Alloy

The supersaturated α solid
solution is usually heated to an
intermediate temperature T2
within the α+β region (diffusion
rates increase).

The β precipitates (PPT) begin
to form as finely dispersed
particles. This process is
referred to as aging.
 After aging at T2, the alloy is
cooled to room temperature.

Strength and hardness of the
alloy depend on the ppt
temperature (T2) and the aging
time at this temperature.
Precipitation Heat Treatment – the 2nd
stage
0 10 20 30 40 50
wt% Cu
L
α+Lα
α+θ
θ
θ+L
300
400
500
600
700
(Al)
T(°C)
composition range
available for precipitation hardening
CuAl2
A
Precipitation Hardening
• Particles impede dislocation motion.
• Ex: Al-Cu system
• Procedure:
-- Pt B: quench to room temp.
(retain α solid solution)
-- Pt C: reheat to nucleate
small θ particles within
α phase.
Temp.
Time
-- Pt A: solution heat treat
(get α solid solution)
Pt A (solution heat treat)
B
Pt B
C
Pt C (precipitate θ)
At room temperature the stable state
of an aluminum-copper alloy is an
aluminum-rich solid solution (α) and
an intermetallic phase with a
tetragonal crystal structure having
nominal composition CuAl2 (θ).
Precipitation Heat Treatment – the 2nd
stage

PPT behavior is represented
in the diagram:

With increasing time, the
hardness increases, reaching
a maximum (peak), then
decreasing in strength.

The reduction in strength and
hardness after long periods is
overaging (continued particle
growth). Small solute-enriched regions in a
solid solution where the lattice is
identical or somewhat perturbed from
that of the solid solution are called
Guinier-Preston zones.
24
• Hard precipitates are difficult to shear.
Ex: Ceramics in metals (SiC in Iron or Aluminum).
Large shear stress needed
to move dislocation toward
precipitate and shear it.
Side View
Top View
Slipped part of slip plane
Unslipped part of slip plane
S
Dislocation
“advances” but
precipitates act as
“pinning” sites with
spacing S.
precipitate
• Result: σy ~
1
S
PRECIPITATION STRENGTHENING
Several stages in the formation of the equilibrium
PPT (θ) phase.
(a)supersaturated α solid solution;
(b)transition (θ”) PPT phase;
(c)equilibrium θ phase within the α matrix phase.
• 2014 Al Alloy:
• TS peak with precipitation time.
• Increasing T accelerates
process.
Influence of Precipitation Heat Treatment on
Tensile Strength (TS), %EL
precipitation heat treat time
tensilestrength(MPa)
200
300
400
100
1min 1h 1day 1mo 1yr
204°C
non-equil.
solidsolution
manysmall
precipitates“aged”
fewerlarge
precipitates
“overaged”
149°C
• %EL reaches minimum
with precipitation time.
%EL(2insample)
10
20
30
0
1min 1h 1day 1mo 1yr
204°C 149°C
precipitation heat treat time
Effects of Temperature

Characteristics of a 2014
aluminum alloy (0.9 wt% Si, 4.4
wt% Cu, 0.8 wt% Mn, 0.5 wt%
Mg) at 4 different aging
temperatures.
Aluminum rivets

Alloys that experience significant
precipitation hardening at room
temp and after short periods must
be quenched to and stored under
refrigerated conditions.

Several aluminum alloys that are
used for rivets exhibit this
behavior. They are driven while
still soft, then allowed to age
harden at the normal room
temperature.

Mais conteúdo relacionado

Mais procurados

Phase transformation edited.ppt1
Phase transformation edited.ppt1Phase transformation edited.ppt1
Phase transformation edited.ppt1Abhijeet Dash
 
Iron Carbon Phase Diagram
Iron Carbon Phase DiagramIron Carbon Phase Diagram
Iron Carbon Phase DiagramJose Surendran
 
CCt Curve (continuos cooling transformation)
CCt Curve (continuos cooling transformation)CCt Curve (continuos cooling transformation)
CCt Curve (continuos cooling transformation)Avinash Navin
 
Jominy end quench hardenability test
Jominy end quench hardenability testJominy end quench hardenability test
Jominy end quench hardenability testTejas Atyam
 
Iron iron carbon equilibrium diagram
Iron iron carbon equilibrium diagramIron iron carbon equilibrium diagram
Iron iron carbon equilibrium diagramRushikesh Raval
 
Iron iron carbide diagram By Hariprasad
Iron iron carbide diagram By HariprasadIron iron carbide diagram By Hariprasad
Iron iron carbide diagram By HariprasadSachin Hariprasad
 
introduction to Cast Iron
introduction to Cast Ironintroduction to Cast Iron
introduction to Cast Ironpulkit bajaj
 
TTT diagram and Heat treatment processes
TTT diagram and Heat treatment processesTTT diagram and Heat treatment processes
TTT diagram and Heat treatment processesSaumy Agarwal
 
Heat treatment of steel
Heat treatment of steelHeat treatment of steel
Heat treatment of steelmeet patel
 
Iron iron carbon dia
Iron iron carbon diaIron iron carbon dia
Iron iron carbon diaKeval Patil
 
Heat treatment part 1
Heat treatment part 1Heat treatment part 1
Heat treatment part 1Naman Dave
 
TTT diagram of eutectoid steel and martensitic transformation
TTT diagram of eutectoid steel and martensitic transformationTTT diagram of eutectoid steel and martensitic transformation
TTT diagram of eutectoid steel and martensitic transformationonlinemetallurgy.com
 
Temperature Time Transformation Diagram (TTT Diagram)
Temperature Time Transformation Diagram (TTT Diagram)Temperature Time Transformation Diagram (TTT Diagram)
Temperature Time Transformation Diagram (TTT Diagram)SAAD ARIF
 

Mais procurados (20)

Phase transformation edited.ppt1
Phase transformation edited.ppt1Phase transformation edited.ppt1
Phase transformation edited.ppt1
 
Iron Carbon Phase Diagram
Iron Carbon Phase DiagramIron Carbon Phase Diagram
Iron Carbon Phase Diagram
 
IRON CARBON EQUILIBRIUM DIAGRAM, TTT DIAGRAM AND HEAT TREATMENT
IRON CARBON EQUILIBRIUM DIAGRAM, TTT DIAGRAM AND HEAT TREATMENTIRON CARBON EQUILIBRIUM DIAGRAM, TTT DIAGRAM AND HEAT TREATMENT
IRON CARBON EQUILIBRIUM DIAGRAM, TTT DIAGRAM AND HEAT TREATMENT
 
CCt Curve (continuos cooling transformation)
CCt Curve (continuos cooling transformation)CCt Curve (continuos cooling transformation)
CCt Curve (continuos cooling transformation)
 
Jominy end quench hardenability test
Jominy end quench hardenability testJominy end quench hardenability test
Jominy end quench hardenability test
 
Microstructures
MicrostructuresMicrostructures
Microstructures
 
Ttt cct diagrams
Ttt cct diagramsTtt cct diagrams
Ttt cct diagrams
 
TTT diagram
TTT diagramTTT diagram
TTT diagram
 
Iron iron carbon equilibrium diagram
Iron iron carbon equilibrium diagramIron iron carbon equilibrium diagram
Iron iron carbon equilibrium diagram
 
Iron iron carbide diagram By Hariprasad
Iron iron carbide diagram By HariprasadIron iron carbide diagram By Hariprasad
Iron iron carbide diagram By Hariprasad
 
introduction to Cast Iron
introduction to Cast Ironintroduction to Cast Iron
introduction to Cast Iron
 
TTT diagram and Heat treatment processes
TTT diagram and Heat treatment processesTTT diagram and Heat treatment processes
TTT diagram and Heat treatment processes
 
Heat Treatment Of Steel
Heat Treatment Of SteelHeat Treatment Of Steel
Heat Treatment Of Steel
 
Iron carbon diagram presentation
Iron carbon diagram presentationIron carbon diagram presentation
Iron carbon diagram presentation
 
Heat treatment of steel
Heat treatment of steelHeat treatment of steel
Heat treatment of steel
 
Iron iron carbon dia
Iron iron carbon diaIron iron carbon dia
Iron iron carbon dia
 
Heat treatment part 1
Heat treatment part 1Heat treatment part 1
Heat treatment part 1
 
Steel Making: Ingot casting defects
Steel Making: Ingot casting defectsSteel Making: Ingot casting defects
Steel Making: Ingot casting defects
 
TTT diagram of eutectoid steel and martensitic transformation
TTT diagram of eutectoid steel and martensitic transformationTTT diagram of eutectoid steel and martensitic transformation
TTT diagram of eutectoid steel and martensitic transformation
 
Temperature Time Transformation Diagram (TTT Diagram)
Temperature Time Transformation Diagram (TTT Diagram)Temperature Time Transformation Diagram (TTT Diagram)
Temperature Time Transformation Diagram (TTT Diagram)
 

Semelhante a Phase transformation physical metallurgy

Power piont ch2 phase-transformation-in-metals (1)
Power piont   ch2 phase-transformation-in-metals (1)Power piont   ch2 phase-transformation-in-metals (1)
Power piont ch2 phase-transformation-in-metals (1)temkin abdlkader
 
ME 3101 Material Science and Engineering Fall 2016
ME 3101 Material Science and Engineering Fall 2016ME 3101 Material Science and Engineering Fall 2016
ME 3101 Material Science and Engineering Fall 2016Savanna Holt
 
tttdiagram-131118222243-phpapp01.pptx
tttdiagram-131118222243-phpapp01.pptxtttdiagram-131118222243-phpapp01.pptx
tttdiagram-131118222243-phpapp01.pptxupender3
 
heat tratment & iron carbon diagram
heat tratment & iron carbon diagramheat tratment & iron carbon diagram
heat tratment & iron carbon diagrammukeshkumar2062
 
Phase transformation (Material Science)
Phase transformation (Material Science)Phase transformation (Material Science)
Phase transformation (Material Science)Myo Zin Aung
 
time temperature transformation
time temperature transformationtime temperature transformation
time temperature transformationHamza Suharwardi
 
Fallsem2021 22 mee1005-eth_vl2021220102807_reference_material_ii_30-aug-2021_...
Fallsem2021 22 mee1005-eth_vl2021220102807_reference_material_ii_30-aug-2021_...Fallsem2021 22 mee1005-eth_vl2021220102807_reference_material_ii_30-aug-2021_...
Fallsem2021 22 mee1005-eth_vl2021220102807_reference_material_ii_30-aug-2021_...RahulRajelli
 
BME 303 - Lesson 7 - Phase Transformation.pdf
BME 303 - Lesson 7 - Phase Transformation.pdfBME 303 - Lesson 7 - Phase Transformation.pdf
BME 303 - Lesson 7 - Phase Transformation.pdfatlestmunni
 
L7_Fe-C_ Diagram MICRO STRUCTURE.pdf
L7_Fe-C_ Diagram MICRO STRUCTURE.pdfL7_Fe-C_ Diagram MICRO STRUCTURE.pdf
L7_Fe-C_ Diagram MICRO STRUCTURE.pdfglorialidwinbdacemec
 
Heat Treating: The How and Why of Quenching Metal Parts
Heat Treating: The How and Why of Quenching Metal PartsHeat Treating: The How and Why of Quenching Metal Parts
Heat Treating: The How and Why of Quenching Metal PartsHoughton International Inc.
 
TIME TEMPERATURE TRANSFORMATION DIAGRAM
TIME TEMPERATURE TRANSFORMATION DIAGRAMTIME TEMPERATURE TRANSFORMATION DIAGRAM
TIME TEMPERATURE TRANSFORMATION DIAGRAMChandra Kumar S
 

Semelhante a Phase transformation physical metallurgy (20)

Power piont ch2 phase-transformation-in-metals (1)
Power piont   ch2 phase-transformation-in-metals (1)Power piont   ch2 phase-transformation-in-metals (1)
Power piont ch2 phase-transformation-in-metals (1)
 
Ch10 m
Ch10 mCh10 m
Ch10 m
 
Ch10
Ch10Ch10
Ch10
 
ME 3101 Material Science and Engineering Fall 2016
ME 3101 Material Science and Engineering Fall 2016ME 3101 Material Science and Engineering Fall 2016
ME 3101 Material Science and Engineering Fall 2016
 
tttdiagram-131118222243-phpapp01.pptx
tttdiagram-131118222243-phpapp01.pptxtttdiagram-131118222243-phpapp01.pptx
tttdiagram-131118222243-phpapp01.pptx
 
heat tratment & iron carbon diagram
heat tratment & iron carbon diagramheat tratment & iron carbon diagram
heat tratment & iron carbon diagram
 
Phase transformation (Material Science)
Phase transformation (Material Science)Phase transformation (Material Science)
Phase transformation (Material Science)
 
Unit 3.pdf
Unit 3.pdfUnit 3.pdf
Unit 3.pdf
 
Phase transitions
Phase transitionsPhase transitions
Phase transitions
 
Fe-C diagram
Fe-C diagramFe-C diagram
Fe-C diagram
 
EMM lecture.ppt
EMM lecture.pptEMM lecture.ppt
EMM lecture.ppt
 
time temperature transformation
time temperature transformationtime temperature transformation
time temperature transformation
 
Fallsem2021 22 mee1005-eth_vl2021220102807_reference_material_ii_30-aug-2021_...
Fallsem2021 22 mee1005-eth_vl2021220102807_reference_material_ii_30-aug-2021_...Fallsem2021 22 mee1005-eth_vl2021220102807_reference_material_ii_30-aug-2021_...
Fallsem2021 22 mee1005-eth_vl2021220102807_reference_material_ii_30-aug-2021_...
 
BME 303 - Lesson 7 - Phase Transformation.pdf
BME 303 - Lesson 7 - Phase Transformation.pdfBME 303 - Lesson 7 - Phase Transformation.pdf
BME 303 - Lesson 7 - Phase Transformation.pdf
 
L7_Fe-C_ Diagram MICRO STRUCTURE.pdf
L7_Fe-C_ Diagram MICRO STRUCTURE.pdfL7_Fe-C_ Diagram MICRO STRUCTURE.pdf
L7_Fe-C_ Diagram MICRO STRUCTURE.pdf
 
IRON CARBON DIAGRAM PPT.pptx
IRON CARBON DIAGRAM PPT.pptxIRON CARBON DIAGRAM PPT.pptx
IRON CARBON DIAGRAM PPT.pptx
 
TTT DIAGRAM
TTT DIAGRAMTTT DIAGRAM
TTT DIAGRAM
 
Heat Treating: The How and Why of Quenching Metal Parts
Heat Treating: The How and Why of Quenching Metal PartsHeat Treating: The How and Why of Quenching Metal Parts
Heat Treating: The How and Why of Quenching Metal Parts
 
TIME TEMPERATURE TRANSFORMATION DIAGRAM
TIME TEMPERATURE TRANSFORMATION DIAGRAMTIME TEMPERATURE TRANSFORMATION DIAGRAM
TIME TEMPERATURE TRANSFORMATION DIAGRAM
 
Ttt diagram
Ttt diagramTtt diagram
Ttt diagram
 

Último

Double Revolving field theory-how the rotor develops torque
Double Revolving field theory-how the rotor develops torqueDouble Revolving field theory-how the rotor develops torque
Double Revolving field theory-how the rotor develops torqueBhangaleSonal
 
Thermal Engineering Unit - I & II . ppt
Thermal Engineering  Unit - I & II . pptThermal Engineering  Unit - I & II . ppt
Thermal Engineering Unit - I & II . pptDineshKumar4165
 
Navigating Complexity: The Role of Trusted Partners and VIAS3D in Dassault Sy...
Navigating Complexity: The Role of Trusted Partners and VIAS3D in Dassault Sy...Navigating Complexity: The Role of Trusted Partners and VIAS3D in Dassault Sy...
Navigating Complexity: The Role of Trusted Partners and VIAS3D in Dassault Sy...Arindam Chakraborty, Ph.D., P.E. (CA, TX)
 
Design For Accessibility: Getting it right from the start
Design For Accessibility: Getting it right from the startDesign For Accessibility: Getting it right from the start
Design For Accessibility: Getting it right from the startQuintin Balsdon
 
Computer Lecture 01.pptxIntroduction to Computers
Computer Lecture 01.pptxIntroduction to ComputersComputer Lecture 01.pptxIntroduction to Computers
Computer Lecture 01.pptxIntroduction to ComputersMairaAshraf6
 
XXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXX
XXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXX
XXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXssuser89054b
 
Kuwait City MTP kit ((+919101817206)) Buy Abortion Pills Kuwait
Kuwait City MTP kit ((+919101817206)) Buy Abortion Pills KuwaitKuwait City MTP kit ((+919101817206)) Buy Abortion Pills Kuwait
Kuwait City MTP kit ((+919101817206)) Buy Abortion Pills Kuwaitjaanualu31
 
A CASE STUDY ON CERAMIC INDUSTRY OF BANGLADESH.pptx
A CASE STUDY ON CERAMIC INDUSTRY OF BANGLADESH.pptxA CASE STUDY ON CERAMIC INDUSTRY OF BANGLADESH.pptx
A CASE STUDY ON CERAMIC INDUSTRY OF BANGLADESH.pptxmaisarahman1
 
Tamil Call Girls Bhayandar WhatsApp +91-9930687706, Best Service
Tamil Call Girls Bhayandar WhatsApp +91-9930687706, Best ServiceTamil Call Girls Bhayandar WhatsApp +91-9930687706, Best Service
Tamil Call Girls Bhayandar WhatsApp +91-9930687706, Best Servicemeghakumariji156
 
School management system project Report.pdf
School management system project Report.pdfSchool management system project Report.pdf
School management system project Report.pdfKamal Acharya
 
PE 459 LECTURE 2- natural gas basic concepts and properties
PE 459 LECTURE 2- natural gas basic concepts and propertiesPE 459 LECTURE 2- natural gas basic concepts and properties
PE 459 LECTURE 2- natural gas basic concepts and propertiessarkmank1
 
A Study of Urban Area Plan for Pabna Municipality
A Study of Urban Area Plan for Pabna MunicipalityA Study of Urban Area Plan for Pabna Municipality
A Study of Urban Area Plan for Pabna MunicipalityMorshed Ahmed Rahath
 
Thermal Engineering -unit - III & IV.ppt
Thermal Engineering -unit - III & IV.pptThermal Engineering -unit - III & IV.ppt
Thermal Engineering -unit - III & IV.pptDineshKumar4165
 
Employee leave management system project.
Employee leave management system project.Employee leave management system project.
Employee leave management system project.Kamal Acharya
 
HAND TOOLS USED AT ELECTRONICS WORK PRESENTED BY KOUSTAV SARKAR
HAND TOOLS USED AT ELECTRONICS WORK PRESENTED BY KOUSTAV SARKARHAND TOOLS USED AT ELECTRONICS WORK PRESENTED BY KOUSTAV SARKAR
HAND TOOLS USED AT ELECTRONICS WORK PRESENTED BY KOUSTAV SARKARKOUSTAV SARKAR
 
Hostel management system project report..pdf
Hostel management system project report..pdfHostel management system project report..pdf
Hostel management system project report..pdfKamal Acharya
 
data_management_and _data_science_cheat_sheet.pdf
data_management_and _data_science_cheat_sheet.pdfdata_management_and _data_science_cheat_sheet.pdf
data_management_and _data_science_cheat_sheet.pdfJiananWang21
 
S1S2 B.Arch MGU - HOA1&2 Module 3 -Temple Architecture of Kerala.pptx
S1S2 B.Arch MGU - HOA1&2 Module 3 -Temple Architecture of Kerala.pptxS1S2 B.Arch MGU - HOA1&2 Module 3 -Temple Architecture of Kerala.pptx
S1S2 B.Arch MGU - HOA1&2 Module 3 -Temple Architecture of Kerala.pptxSCMS School of Architecture
 

Último (20)

Double Revolving field theory-how the rotor develops torque
Double Revolving field theory-how the rotor develops torqueDouble Revolving field theory-how the rotor develops torque
Double Revolving field theory-how the rotor develops torque
 
Thermal Engineering Unit - I & II . ppt
Thermal Engineering  Unit - I & II . pptThermal Engineering  Unit - I & II . ppt
Thermal Engineering Unit - I & II . ppt
 
Navigating Complexity: The Role of Trusted Partners and VIAS3D in Dassault Sy...
Navigating Complexity: The Role of Trusted Partners and VIAS3D in Dassault Sy...Navigating Complexity: The Role of Trusted Partners and VIAS3D in Dassault Sy...
Navigating Complexity: The Role of Trusted Partners and VIAS3D in Dassault Sy...
 
Design For Accessibility: Getting it right from the start
Design For Accessibility: Getting it right from the startDesign For Accessibility: Getting it right from the start
Design For Accessibility: Getting it right from the start
 
Computer Lecture 01.pptxIntroduction to Computers
Computer Lecture 01.pptxIntroduction to ComputersComputer Lecture 01.pptxIntroduction to Computers
Computer Lecture 01.pptxIntroduction to Computers
 
XXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXX
XXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXX
XXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXX
 
Kuwait City MTP kit ((+919101817206)) Buy Abortion Pills Kuwait
Kuwait City MTP kit ((+919101817206)) Buy Abortion Pills KuwaitKuwait City MTP kit ((+919101817206)) Buy Abortion Pills Kuwait
Kuwait City MTP kit ((+919101817206)) Buy Abortion Pills Kuwait
 
A CASE STUDY ON CERAMIC INDUSTRY OF BANGLADESH.pptx
A CASE STUDY ON CERAMIC INDUSTRY OF BANGLADESH.pptxA CASE STUDY ON CERAMIC INDUSTRY OF BANGLADESH.pptx
A CASE STUDY ON CERAMIC INDUSTRY OF BANGLADESH.pptx
 
Tamil Call Girls Bhayandar WhatsApp +91-9930687706, Best Service
Tamil Call Girls Bhayandar WhatsApp +91-9930687706, Best ServiceTamil Call Girls Bhayandar WhatsApp +91-9930687706, Best Service
Tamil Call Girls Bhayandar WhatsApp +91-9930687706, Best Service
 
School management system project Report.pdf
School management system project Report.pdfSchool management system project Report.pdf
School management system project Report.pdf
 
PE 459 LECTURE 2- natural gas basic concepts and properties
PE 459 LECTURE 2- natural gas basic concepts and propertiesPE 459 LECTURE 2- natural gas basic concepts and properties
PE 459 LECTURE 2- natural gas basic concepts and properties
 
A Study of Urban Area Plan for Pabna Municipality
A Study of Urban Area Plan for Pabna MunicipalityA Study of Urban Area Plan for Pabna Municipality
A Study of Urban Area Plan for Pabna Municipality
 
Thermal Engineering -unit - III & IV.ppt
Thermal Engineering -unit - III & IV.pptThermal Engineering -unit - III & IV.ppt
Thermal Engineering -unit - III & IV.ppt
 
Employee leave management system project.
Employee leave management system project.Employee leave management system project.
Employee leave management system project.
 
HAND TOOLS USED AT ELECTRONICS WORK PRESENTED BY KOUSTAV SARKAR
HAND TOOLS USED AT ELECTRONICS WORK PRESENTED BY KOUSTAV SARKARHAND TOOLS USED AT ELECTRONICS WORK PRESENTED BY KOUSTAV SARKAR
HAND TOOLS USED AT ELECTRONICS WORK PRESENTED BY KOUSTAV SARKAR
 
FEA Based Level 3 Assessment of Deformed Tanks with Fluid Induced Loads
FEA Based Level 3 Assessment of Deformed Tanks with Fluid Induced LoadsFEA Based Level 3 Assessment of Deformed Tanks with Fluid Induced Loads
FEA Based Level 3 Assessment of Deformed Tanks with Fluid Induced Loads
 
Hostel management system project report..pdf
Hostel management system project report..pdfHostel management system project report..pdf
Hostel management system project report..pdf
 
data_management_and _data_science_cheat_sheet.pdf
data_management_and _data_science_cheat_sheet.pdfdata_management_and _data_science_cheat_sheet.pdf
data_management_and _data_science_cheat_sheet.pdf
 
Cara Menggugurkan Sperma Yang Masuk Rahim Biyar Tidak Hamil
Cara Menggugurkan Sperma Yang Masuk Rahim Biyar Tidak HamilCara Menggugurkan Sperma Yang Masuk Rahim Biyar Tidak Hamil
Cara Menggugurkan Sperma Yang Masuk Rahim Biyar Tidak Hamil
 
S1S2 B.Arch MGU - HOA1&2 Module 3 -Temple Architecture of Kerala.pptx
S1S2 B.Arch MGU - HOA1&2 Module 3 -Temple Architecture of Kerala.pptxS1S2 B.Arch MGU - HOA1&2 Module 3 -Temple Architecture of Kerala.pptx
S1S2 B.Arch MGU - HOA1&2 Module 3 -Temple Architecture of Kerala.pptx
 

Phase transformation physical metallurgy

  • 1. Chapter 11 Phase TransformationsFe3C (cementite)- orthorhombic Martensite - BCT Austenite - FCC Ferrite - BCC
  • 2. Phase Transformations • Transformation rate • Kinetics of Phase Transformation –Nucleation: homogeneous, heterogeneous –Free Energy, Growth • Isothermal Transformations (TTT diagrams) • Pearlite, Martensite, Spheroidite, Bainite • Continuous Cooling • Mechanical Behavior • Precipitation Hardening
  • 3. Phase Transformations  Phase transformations – change in the number or character of phases.  Simple diffusion-dependent  No change in # of phases  No change in composition  Example: solidification of a pure metal, allotropic transformation, recrystallization, grain growth  More complicated diffusion-dependent  Change in # of phases  Change in composition  Example: eutectoid reaction  Diffusionless  Example: metastable phase - martensite
  • 4. Phase Transformations  Most phase transformations begin with the formation of numerous small particles of the new phase that increase in size until the transformation is complete. • Nucleation is the process whereby nuclei (seeds) act as templates for crystal growth. • Homogeneous nucleation - nuclei form uniformly throughout the parent phase; requires considerable supercooling (typically 80-300°C). • Heterogeneous nucleation - form at structural inhomogeneities (container surfaces, impurities, grain boundaries, dislocations) in liquid phase much easier since stable “nucleating surface” is already present; requires slight supercooling (0.1-10ºC).
  • 5. Supercooling  During the cooling of a liquid, solidification (nucleation) will begin only after the temperature has been lowered below the equilibrium solidification (or melting) temperature Tm. This phenomenon is termed supercooling (or undercooling.  The driving force to nucleate increases as ∆T increases  Small supercooling  slow nucleation rate - few nuclei - large crystals  Large supercooling  rapid nucleation rate - many nuclei - small crystals
  • 6. Nucleation of a spherical solid particle in a liquid Liquid  The change in free energy ∆G (a function of the internal energy and enthalpy of the system) must be negative for a transformation to occur.  Assume that nuclei of the solid phase form in the interior of the liquid as atoms cluster together- similar to the packing in the solid phase.  Also, each nucleus is spherical and has a radius r.  Free energy changes as a result of a transformation: 1) the difference between the solid and liquid phases (volume free energy, ∆GV); and 2) the solid-liquid phase boundary (surface free energy, ∆GS).  Transforming one phase into another takes time. ∆G = ∆GS + ∆GV Fe γ (Austenite) Eutectoid transformation C FCC Fe3C (cementite) α (ferrite) + (BCC)
  • 7. r* = critical nucleus: for r < r* nuclei shrink; for r >r* nuclei grow (to reduce energy) Homogeneous Nucleation & Energy Effects ∆GT = Total Free Energy = ∆GS + ∆GV Surface Free Energy- destabilizes the nuclei (it takes energy to make an interface) γπ=∆ 2 4 rGS γ = surface tension Volume (Bulk) Free Energy – stabilizes the nuclei (releases energy) υ∆π=∆ GrGV 3 3 4 volumeunit energyfreevolume =∆ υG
  • 8. Solidification TH T r f m ∆∆ γ− = 2 * Note: ∆Hf and γ are weakly dependent on ∆T ∴ r* decreases as ∆T increases For typical ∆T r* ~ 10 nm ∆Hf = latent heat of solidification (fusion) Tm = melting temperature γ = surface free energy ∆T = Tm - T = supercooling r* = critical radius
  • 9. Transformations & Undercooling • For transformation to occur, must cool to below 727°C • Eutectoid transformation (Fe-Fe3C system): γ ⇒ α + Fe3C 0.76 wt% C 0.022 wt% C 6.7 wt% C Fe3C(cementite) 1600 1400 1200 1000 800 600 400 0 1 2 3 4 5 6 6.7 L γ (austenite) γ+L γ +Fe3C α +Fe3C L+Fe3C δ (Fe) C, wt% C 1148°C T(°C) α ferrite 727°C Eutectoid: Equil. Cooling: Ttransf. = 727ºC ∆T Undercooling by Ttransf. < 727°C 0.76 0.022
  • 10. 2 • Fraction transformed depends on time. fraction transformed time y = 1− e −ktn Avrami Eqn. • Transformation rate depends on T. 1 10 102 1040 50 100 135°C 119°C113°C102°C 88°C 43°C y (%) log (t) min Ex: recrystallization of Cu r = 1 t 0.5 = Ae −Q /RT activation energy • r often small: equil not possible y log (t) Fixed T 0 0.5 1 t0.5 FRACTION OF TRANSFORMATION
  • 11. Generation of Isothermal Transformation Diagrams • The Fe-Fe3C system, for Co = 0.76 wt% C • A transformation temperature of 675°C. 100 50 0 1 102 104 T = 675°C %transformed time (s) 400 500 600 700 1 10 102 103 104 105 0%pearlite 100% 50% Austenite (stable) TE (727°C)Austenite (unstable) Pearlite T(°C) time (s) isothermal transformation at 675°C Consider:
  • 12. Coarse pearlite  formed at higher temperatures – relatively soft Fine pearlite  formed at lower temperatures – relatively hard • Transformation of austenite to pearlite: γα α α α α α pearlite growth direction Austenite (γ) grain boundary cementite (Fe3C) Ferrite (α) γ • For this transformation, rate increases with ( ∆T) [Teutectoid – T ]. 675°C (∆T smaller) 0 50 %pearlite 600°C (∆T larger) 650°C 100 Diffusion of C during transformation α α γ γ α Carbon diffusion Eutectoid Transformation Rate ~ ∆T
  • 13. 5 • Reaction rate is a result of nucleation and growth of crystals. • Examples: % Pearlite 0 50 100 Nucleation regime Growth regime log (time)t50 Nucleation rate increases w/ ∆T Growth rate increases w/ T Nucleation rate high T just below TE T moderately below TE T way below TE Nucleation rate low Growth rate high γ γ γ pearlite colony Nucleation rate med . Growth rate med. Growth rate low Nucleation and Growth
  • 14. Isothermal Transformation Diagrams 2 solid curves are plotted:  one represents the time required at each temperature for the start of the transformation;  the other is for transformation completion.  The dashed curve corresponds to 50% completion. The austenite to pearlite transformation will occur only if the alloy is supercooled to below the eutectoid temperature (727˚C). Time for process to complete depends on the temperature.
  • 15. • Eutectoid iron-carbon alloy; composition, Co = 0.76 wt% C • Begin at T > 727˚C • Rapidly cool to 625˚C and hold isothermally. Isothermal Transformation Diagram Austenite-to-Pearlite
  • 16. Transformations Involving Noneutectoid Compositions Hypereutectoid composition – proeutectoid cementite Consider C0 = 1.13 wt% C Fe3C(cementite) 1600 1400 1200 1000 800 600 400 0 1 2 3 4 5 6 6.7 L γ (austenite) γ+L γ +Fe3C α+Fe3C L+Fe3C δ (Fe) C, wt%C T(°C) 727°C ∆T 0.76 0.022 1.13
  • 17. Strength Ductility Martensite T Martensite bainite fine pearlite coarse pearlite spheroidite General Trends Possible Transformations
  • 18. Coarse pearlite (high diffusion rate) and (b) fine pearlite - Smaller ∆T: colonies are larger - Larger ∆T: colonies are smaller
  • 19. 10 103 105 time (s) 10-1 400 600 800 T(°C) Austenite (stable) 200 P B TE 0% 100% 50% A A Bainite: Non-Equil Transformation Products  elongated Fe3C particles in α-ferrite matrix  diffusion controlled  α lathes (strips) with long rods of Fe3C 100% bainite 100% pearlite Martensite Cementite Ferrite
  • 20. Bainite Microstructure • Bainite consists of acicular (needle-like) ferrite with very small cementite particles dispersed throughout. • The carbon content is typically greater than 0.1%. • Bainite transforms to iron and cementite with sufficient time and temperature (considered semi-stable below 150°C).
  • 21. 10  Fe3C particles within an α-ferrite matrix  diffusion dependent  heat bainite or pearlite at temperature just below eutectoid for long times  driving force – reduction of α-ferrite/Fe3C interfacial area Spheroidite: Nonequilibrium Transformation 10 103 105time (s)10-1 400 600 800 T(°C) Austenite (stable) 200 P B TE 0% 100% 50% A A Spheroidite 100% spheroidite 100% spheroidite
  • 22. Pearlitic Steel partially transformed to Spheroidite
  • 23.  single phase  body centered tetragonal (BCT) crystal structure  BCT if C0 > 0.15 wt% C  Diffusionless transformation  BCT  few slip planes  hard, brittle  % transformation depends only on T of rapid cooling Martensite Formation • Isothermal Transformation Diagram 10 10 3 10 5 time (s)10 -1 400 600 800 T(°C) Austenite (stable) 200 P B TE 0% 100%50% A A M + A M + A M + A 0% 50% 90% Martensite needles Austenite
  • 24. An micrograph of austenite that was polished flat and then allowed to transform into martensite. The different colors indicate the displacements caused when martensite forms.
  • 25. Isothermal Transformation Diagram Iron-carbon alloy with eutectoid composition.  A: Austenite  P: Pearlite  B: Bainite  M: Martensite
  • 26.  Other elements (Cr, Ni, Mo, Si and W) may cause significant changes in the positions and shapes of the TTT curves:  Change transition temperature;  Shift the nose of the austenite-to- pearlite transformation to longer times;  Shift the pearlite and bainite noses to longer times (decrease critical cooling rate);  Form a separate bainite nose; Effect of Adding Other Elements 4340 Steel plain carbon steel nose  Plain carbon steel: primary alloying element is carbon.
  • 27. Example 11.2:  Iron-carbon alloy with eutectoid composition.  Specify the nature of the final microstructure (% bainite, martensite, pearlite etc) for the alloy that is subjected to the following time–temperature treatments:  Alloy begins at 760˚C and has been held long enough to achieve a complete and homogeneous austenitic structure. Treatment (a)  Rapidly cool to 350 ˚C  Hold for 104 seconds  Quench to room temperature Bainite, 100%
  • 28. Martensite, 100% Example 11.2:  Iron-carbon alloy with eutectoid composition.  Specify the nature of the final microstructure (% bainite, martensite, pearlite etc) for the alloy that is subjected to the following time–temperature treatments:  Alloy begins at 760˚C and has been held long enough to achieve a complete and homogeneous austenitic structure. Treatment (b)  Rapidly cool to 250 ˚C  Hold for 100 seconds  Quench to room temperature Austenite, 100%
  • 29. Bainite, 50% Example 11.2:  Iron-carbon alloy with eutectoid composition.  Specify the nature of the final microstructure (% bainite, martensite, pearlite etc) for the alloy that is subjected to the following time–temperature treatments:  Alloy begins at 760˚C and has been held long enough to achieve a complete and homogeneous austenitic structure. Treatment (c)  Rapidly cool to 650˚C  Hold for 20 seconds  Rapidly cool to 400˚C  Hold for 103 seconds  Quench to room temperature Austenite, 100% Almost 50% Pearlite, 50% Austenite Final: 50% Bainite, 50% Pearlite
  • 30. Continuous Cooling Transformation Diagrams  Isothermal heat treatments are not the most practical due to rapidly cooling and constant maintenance at an elevated temperature.  Most heat treatments for steels involve the continuous cooling of a specimen to room temperature.  TTT diagram (dotted curve) is modified for a CCT diagram (solid curve).  For continuous cooling, the time required for a reaction to begin and end is delayed.  The isothermal curves are shifted to longer times and lower temperatures.
  • 31.  Moderately rapid and slow cooling curves are superimposed on a continuous cooling transformation diagram of a eutectoid iron- carbon alloy.  The transformation starts after a time period corresponding to the intersection of the cooling curve with the beginning reaction curve and ends upon crossing the completion transformation curve.  Normally bainite does not form when an alloy is continuously cooled to room temperature; austenite transforms to pearlite before bainite has become possible.  The austenite-pearlite region (A---B) terminates just below the nose. Continued cooling (below Mstart) of austenite will form martensite.
  • 32.  For continuous cooling of a steel alloy there exists a critical quenching rate that represents the minimum rate of quenching that will produce a totally martensitic structure.  This curve will just miss the nose where pearlite transformation begins
  • 33.  Continuous cooling diagram for a 4340 steel alloy and several cooling curves superimposed.  This demonstrates the dependence of the final microstructure on the transformations that occur during cooling.  Alloying elements used to modify the critical cooling rate for martensite are chromium, nickel, molybdenum, manganese, silicon and tungsten.
  • 34. Mechanical Properties • Hardness • Brinell, Rockwell • Yield Strength • Tensile Strength • Ductility • % Elongation • Effect of Carbon Content
  • 35. Mechanical Properties: Influence of Carbon Content C0 > 0.76 wt% C Hypereutectoid Pearlite (med) Cementite (hard) C0 < 0.76 wt% C Hypoeutectoid Pearlite (med) ferrite (soft)
  • 37.  Tempered martensite is less brittle than martensite; tempered at 594 °C.  Tempering reduces internal stresses caused by quenching.  The small particles are cementite; the matrix is α-ferrite. US Steel Corp. Tempered Martensite 4340 steel
  • 38. Hardness as a function of carbon concentration for steels
  • 39. Hardness versus tempering time for a water-quenched eutectoid plain carbon steel (1080); room temperature. Rockwell C and Brinell Hardness
  • 40.
  • 41. Precipitation Hardening • The strength and hardness of some metal alloys may be improved by the formation of extremely small, uniformly dispersed particles (precipitates) of a second phase within the original phase matrix. • Other alloys that can be precipitation hardened or age hardened:  Copper-beryllium (Cu-Be)  Copper-tin (Cu-Sn)  Magnesium-aluminum (Mg-Al)  Aluminum-copper (Al-Cu)  High-strength aluminum alloys
  • 42. Criteria:  Maximum solubility of 1 component in the other (M);  Solubility limit that rapidly decreases with decrease in temperature (M→N). Process:  Solution Heat Treatment – first heat treatment where all solute atoms are dissolved to form a single-phase solid solution. Heat to T0 and dissolve B phase. Rapidly quench to T1  Nonequilibrium state (α phase solid solution supersaturated with B atoms; alloy is soft, weak-no ppts). Phase Diagram for Precipitation Hardened Alloy
  • 43.  The supersaturated α solid solution is usually heated to an intermediate temperature T2 within the α+β region (diffusion rates increase).  The β precipitates (PPT) begin to form as finely dispersed particles. This process is referred to as aging.  After aging at T2, the alloy is cooled to room temperature.  Strength and hardness of the alloy depend on the ppt temperature (T2) and the aging time at this temperature. Precipitation Heat Treatment – the 2nd stage
  • 44. 0 10 20 30 40 50 wt% Cu L α+Lα α+θ θ θ+L 300 400 500 600 700 (Al) T(°C) composition range available for precipitation hardening CuAl2 A Precipitation Hardening • Particles impede dislocation motion. • Ex: Al-Cu system • Procedure: -- Pt B: quench to room temp. (retain α solid solution) -- Pt C: reheat to nucleate small θ particles within α phase. Temp. Time -- Pt A: solution heat treat (get α solid solution) Pt A (solution heat treat) B Pt B C Pt C (precipitate θ) At room temperature the stable state of an aluminum-copper alloy is an aluminum-rich solid solution (α) and an intermetallic phase with a tetragonal crystal structure having nominal composition CuAl2 (θ).
  • 45. Precipitation Heat Treatment – the 2nd stage  PPT behavior is represented in the diagram:  With increasing time, the hardness increases, reaching a maximum (peak), then decreasing in strength.  The reduction in strength and hardness after long periods is overaging (continued particle growth). Small solute-enriched regions in a solid solution where the lattice is identical or somewhat perturbed from that of the solid solution are called Guinier-Preston zones.
  • 46. 24 • Hard precipitates are difficult to shear. Ex: Ceramics in metals (SiC in Iron or Aluminum). Large shear stress needed to move dislocation toward precipitate and shear it. Side View Top View Slipped part of slip plane Unslipped part of slip plane S Dislocation “advances” but precipitates act as “pinning” sites with spacing S. precipitate • Result: σy ~ 1 S PRECIPITATION STRENGTHENING
  • 47. Several stages in the formation of the equilibrium PPT (θ) phase. (a)supersaturated α solid solution; (b)transition (θ”) PPT phase; (c)equilibrium θ phase within the α matrix phase.
  • 48. • 2014 Al Alloy: • TS peak with precipitation time. • Increasing T accelerates process. Influence of Precipitation Heat Treatment on Tensile Strength (TS), %EL precipitation heat treat time tensilestrength(MPa) 200 300 400 100 1min 1h 1day 1mo 1yr 204°C non-equil. solidsolution manysmall precipitates“aged” fewerlarge precipitates “overaged” 149°C • %EL reaches minimum with precipitation time. %EL(2insample) 10 20 30 0 1min 1h 1day 1mo 1yr 204°C 149°C precipitation heat treat time
  • 49. Effects of Temperature  Characteristics of a 2014 aluminum alloy (0.9 wt% Si, 4.4 wt% Cu, 0.8 wt% Mn, 0.5 wt% Mg) at 4 different aging temperatures.
  • 50. Aluminum rivets  Alloys that experience significant precipitation hardening at room temp and after short periods must be quenched to and stored under refrigerated conditions.  Several aluminum alloys that are used for rivets exhibit this behavior. They are driven while still soft, then allowed to age harden at the normal room temperature.