Inspection of MDPE Pipe
SCOPE
IS 14885 covers the requirements for polyethylene pipe from dia. 16
mm to 630 mm with SDR 9,11,14 and 17.6 and in material grade PE-80
& PE- 100.
• Raw Material
• Inspection
Raw material inspection
In Process Inspection
Final Inspection
RAW MATERIAL
CRP 100 Orange - CRP 100 orange is a high density polyethylene, The
product is used for PE 100 and provides excellent stress crack resistance
properties (ESCR) with very good long term hydrostatic strength.
PE 100 XSC50 - It is a high performance hexene based orange compound,
with a MRS 10 MPa.
Eltex TUB 125 N2025- Eltex TUB 125 N2025 is a high-density polyethylene
copolymer designed for the extrusion of pipes for gas applications.
HE3492 LSH- It is used to ensure excellent long-term thermal stability and
UV-resistance.
INSPECTION
•RAW MATERIAL INSPECTION
•IN PROCESS INSPECTION
•FINAL INSPECTION
RAW MATERIAL INSPECTION
•Density Test
•Melt Flow Rate
•Thermal Stability (OIT)
•Pigment Dispersion
•Volatile Matter Content
DENSITY
IS 14885, CL.-8.3, IS 7328, ANNEX-A
• The density is determine by the buoyancy method by finding the mass
in air and mass in butyl acetate.
• Apparatus-
Analytical balance, butyl acetate, hydrometer, beaker
• Test sample- Weight- 50gm
• Calculation –
Density of PE (KG/M³) = a1*ρ*100/(a1-a2)
a1 - Mass of specimen in air (gm)
a2- Mass of specimen in butyl acetate (gm)
ρ- Density of butyl acetate (0.877 KG/M³)
• Density of butyl acetate determined by hydrometer.
Density of pe should be ≥928.4 KG/M³ @23℃ & ≥ 𝟗𝟑𝟎 KG/M³ @27℃.
PPT on Mdpe inspection.pptx
MELT FLOW RATE (MFR)
(IS 14885, CL.- 8.4, IS 2530)
• Melt Flow Rate measures the rate of extrusion of
thermoplastics through MFT at given temperature and
load.
• It provides measuring flow of a melted material which can
be used to differentiate grades of pipes.
• Sample size –
5 gm. @190℃ , min. 3 nos. sample required
Weight (Load) – 5kg.
• Calculation-
MFR=m*600/t for gm/10 min.
m - avg. mass of minimum 3 nos. sample.
t - cut off time (240 sec.)
• MFR of the compound material shall be ±20%.
MELT FLOW TESTER
Thermal Stability (OIT)
(IS 14885, CL.-8.5, ANNEX-D)
OIT (oxidation induction time) is a type of
test/method to measures the level of thermal
stabilization or oxidation induction time of the pe
material. The time between melting and the
decomposition is measured. The atmosphere is
nitrogen up to melting and then oxygen.
- For long term strength
- Stability of material
- For electrofusion jointing w.r.t. temperature.
Sample size- 15 mg
Test temperature - 200℃
Gas flow of N2 & O2 – 50CM³/min.
Thermal analyser equipment used for this test
OIT ≥ 𝟐𝟎 𝑴𝑰𝑵𝑼𝑻𝑬𝑺 @𝟐𝟎𝟎℃
PIGMENT DISPERSION
(IS 14885, CL.- 5.4, ANNEX-E)
The test is perform to check the proper dispersion in PE material.
Apparatus-
Microscope of at X 100 linear magnification.
Microtome
Hot plate
Test specimen-
Six test pieces shall be taken from different parts of the cross-section.
Thickness & Area of specimen- 10𝜇𝑚 to 20𝜇𝑚 & 7 mm²
Weight – 5 mg
Principle- A microtomed section of material is examined by transmitted light at a magnification of X
100 and compared against standard photomicrographs.
Acceptance- The grading should be ≤ 3.
→ → →
↓
← ← ←
Volatile matter content
(IS 14885, CL.- 8.6, ANNEX-H)
• Volatile matter is an unstable material. Volatile matter tends to
not remain in one state and will rapidly transition to another
state, or vaporize, when the right conditions are met.
• The volatile content is determined as the loss of mass of a
sample, which has been put in a drying oven.
• Calculation – V=(P1-P2)10^6/(P1-P0)
V- volatile matter content (mg/kg)
P0- weight of empty weighing cup (dia. 35mm) in gm.
P1- weight of weighing cup & sample
P2- weight of weighing cup and sample after 1 hr @105℃
Sample size- 25 gm.
Volatile matter content should be ≤ 𝟑𝟓𝟎
𝒎𝒈
𝒌𝒈
In Process Inspection
• Colour
• Finish Of Pipe
• Outside Diameter
• Wall Thickness
• Ovality
• Marking
• Length
Colour
The colour of the pipes shall be
yellow when manufactured from
PE-80 grade and orange from PE-
1OOgrade.
Colour coding confirm with BS
5252
PE 100 – CODE 08 E 55
PE 80 – CODE 08 E 53
Finish of Pipe
• Smooth
• Clean
• Free from grooves
• The ends shall be cleanly cut and shall
be square with axis.
• Considerable “Out of Square
Tolerance of End”-
2mm for 16 to 90mm dia.
3mm for 90 to 140mm dia.
4mm for 140 to 200mm dia.
Outside dia.
Wall thickness
• Negative tolerance should not
allowed during inspection of pipe.
• Ball ended micrometer used to
check the thickness.
• Acceptable plus tolerance-
Table 4 & 5 of IS 14885
PPT on Mdpe inspection.pptx
Ovality
•
Marking
• All pipes shall be permanently marked along
their length with a legend, which shall be
impressed to a depth of not more than 0.2
mm.
• Marking details shall be formed on the pipe
in such away that the marking does not
initiate cracks or other type of failure.
• The embossing for yellow/ orange pipe shall
have black Colour. The height of the
character shall be uniform and at least 3 mm
for ≤ 90𝑚𝑚 & 5 mm for ≥90mm.
• The legend shall be repeated at intervals of 1
m .
• Manufacturer’s name, Designation and Batch
or lot number.
• Each pipe may also be marked with the
Standard Mark.
PPT on Mdpe inspection.pptx
Length
• PE 100 DN 20MM SDR 11
– 200 MTRS.
• PE 100 DN 32MM SDR 11
– 200 MTRS.
• PE 100 DN 63 MM SDR 11
– 100 MTRS.
• PE 100 DN 125 MM SDR
17.6- 50 MTRS.
Final Inspection
•Hydraulic Pressure Resistance Test
•Reversion
•Tensile test (Tensile Strength at Yield &
Elongation at Break)
•Resistance to weathering (Exposure to sunlight)
•Supply, Packaging, Handling & Transportation
Hydraulic Pressure Resistance Test
(IS 14885, CL. 8.1, ANNEX-A&B, TABLE -7)
• When specimen subjected to internal pressure as per given procedure, sample shall show no sign of swelling, leakage, burst or any type of
physical damage.
• TEST SPECIMAN –
Sample taken after 24 hrs. of manufacturing.
Size- 10*OD (250mm to 750mm).
For < ∅63𝑚𝑚 → @80℃ for 165 hrs.→ 5.5 Mpa (induced stress)
For ≥ ∅63𝑚𝑚 → @80℃ for 165 hrs.→ 4.6 Mpa (induced stress)
• Calculation –
Test Pressure (in MPA)=2
𝜎𝑠
𝑑−𝑠
𝜎 − 𝑖𝑛𝑑𝑢𝑠𝑒𝑑 𝑠𝑡𝑟𝑒𝑠𝑠 𝑇𝑎𝑏𝑙𝑒 − 7
s – minimum wall thickness
d – outside dia.
Conclusion - sample shall show no sign of swelling, leakage, burst
Or any Damage during test perform @ above given condition
https://www.youtube.com/watch?v=0qD05rWK39g
Hot water bath Test Sample
PPT on Mdpe inspection.pptx
REVERSION (Shrinkage Or Expansion)
(IS 14885, CL. 8.2)
• The test is performed to check the shrinkage or
expansion of pipe.
• Apparatus-
Hot air circulating oven (@110℃)
Vernier caliper
Glass plate
Talcum powder
• Test specimen-
Size- 200mm for ≤ 200𝑚𝑚 & Axial arc of 200mm for ≥ 200𝑚𝑚
No. of sample – ≥ 3
• Calculation-
Reversion (%)= (Li-Lf)*100/Li
• Conclusion- Value should be in b/w of +3 and -3 in percentage.
Hot air circulating oven
Tensile test-
(IS 14885, CL. 8.7, 8.1, CL.-06 OF IS 2530)
• Tensile yield strength & Elongation at break test of mdpe.
• Test speciman-
Use a sufficiently long piece of pipe, and divide its circumference into a certain number of sectors with
an arc length of 150 mm.
For thickness of specimen- < 5𝑚𝑚 → @ 23°C & 100 mm/min
≥ 5𝑚𝑚 → @ 23°C & 25 mm/min
• Apparatus –
Universal tensile tester
• Procedure- The test pieces shall be conditioned for two hours in air or one hour in water so that it is at
a temperature of 27°C immediately before test.
• Acceptance- Tensile yield strength 15 Mpa
Elongation at break 350 percent, Min
PPT on Mdpe inspection.pptx
→ ¬
← ←
Resistance to weathering (Exposure to sunlight)
(IS 14885, CL.-8.8, ANNEX-F)
• Test specimen –
Length – 1 mtr.
0.2 mm upper layer of specimen shall be remove before testing.
• Time period –
Sample shall be exposed for a period of six months.
The size of the apparatus and the distance between the specimens shall be such that no
shadows fall across the specimens for the period of at least 8 h during which the sun is
normally the strongest.
• Acceptance-
Elongation as per 8.7.1
Hydraulic characteristics as per 8.1
Thermal stability to oxidation as per 8.5
Supply, Packaging, Handling & Transportation
(IS 14885, CL. 11, ANNEX-K)
• SUPPLY-
 The polyethylene pipes shall be supplied as straight length either independent or bundled together.
 Pipe ends shall be cleanly cut, square with the axis of pipe and with appropriate end caps
• Coils-
Polyethylene pipes may be coiled or packed on drums. Large diameter coils with d> 90 mm should be stored flat or vertically.
• Coil Dimension and Winding Temperature-
Size Minimum internal dia Max. external coil dia
20/25 mm 0.6 m 3.2 m
32 mm 0.7 m 3.2 m
63 mm 1.3 m 3.2 m
125 mm 2.5 m 3.2 m
Maximum external surface temperature at time of coiling- 35℃
• All the coils shall be wrapped with PP woven sack & PE film.
PPT on Mdpe inspection.pptx
THANK YOU
Himanshu shukla
1 de 36

Recomendados

C&I Cables TestsC&I Cables Tests
C&I Cables TestsPratyusha Khandelwal
2.3K visualizações28 slides
C&I Cables TestsC&I Cables Tests
C&I Cables TestsPratyusha Khandelwal
505 visualizações28 slides
Lv cable is_694Lv cable is_694
Lv cable is_694vjsudarshan
122 visualizações19 slides
Lv cable is_694Lv cable is_694
Lv cable is_694vjsudarshan
79 visualizações19 slides

Mais conteúdo relacionado

Similar a PPT on Mdpe inspection.pptx

Synopsis 21st februarySynopsis 21st february
Synopsis 21st februaryAnil Venkata Nag Kothur
50 visualizações77 slides
COMPANY PROFILECOMPANY PROFILE
COMPANY PROFILESmileNetCafe1
42 visualizações17 slides
1.2_Basic Engineering_Day 4.pptx1.2_Basic Engineering_Day 4.pptx
1.2_Basic Engineering_Day 4.pptxJanak82
6 visualizações21 slides

Similar a PPT on Mdpe inspection.pptx(20)

Quality Control- Timber & Structural SteelQuality Control- Timber & Structural Steel
Quality Control- Timber & Structural Steel
Pawan Kumar263 visualizações
Synopsis 21st februarySynopsis 21st february
Synopsis 21st february
Anil Venkata Nag Kothur50 visualizações
COMPANY PROFILECOMPANY PROFILE
COMPANY PROFILE
SmileNetCafe142 visualizações
Piping Hydrostatic Test / HydrotestingPiping Hydrostatic Test / Hydrotesting
Piping Hydrostatic Test / Hydrotesting
Abhijeet Nagle4.5K visualizações
1.2_Basic Engineering_Day 4.pptx1.2_Basic Engineering_Day 4.pptx
1.2_Basic Engineering_Day 4.pptx
Janak826 visualizações
Instrumentation Needle Valves | SealexcelInstrumentation Needle Valves | Sealexcel
Instrumentation Needle Valves | Sealexcel
jackmethyu29 visualizações
Penetration of bitumiousPenetration of bitumious
Penetration of bitumious
Taha Samir207 visualizações
INDUSTRIAL TRAINING PRESENTATION aweenINDUSTRIAL TRAINING PRESENTATION aween
INDUSTRIAL TRAINING PRESENTATION aween
Nurul Azwin Mazlan326 visualizações
thermal_properties..pptthermal_properties..ppt
thermal_properties..ppt
RajeshKumarTiwari1859 visualizações
AIAA Presentation Jan 2017AIAA Presentation Jan 2017
AIAA Presentation Jan 2017
Jarrod Buffy470 visualizações
Testing for analysis and quality assuranceTesting for analysis and quality assurance
Testing for analysis and quality assurance
Sylvin Technologies, Inc635 visualizações
Tampere Wear Center & Research equipment 2014Tampere Wear Center & Research equipment 2014
Tampere Wear Center & Research equipment 2014
Kati Valtonen2.1K visualizações
Unit 2 a) Dielectric Breakdown   b) Testing of MaterialUnit 2 a) Dielectric Breakdown   b) Testing of Material
Unit 2 a) Dielectric Breakdown b) Testing of Material
rajendra purkar155 visualizações
Fujikura mechanical splicerFujikura mechanical splicer
Fujikura mechanical splicer
Agus Riyadi442 visualizações
SMC(FRP) Valve Catalogue1SMC(FRP) Valve Catalogue1
SMC(FRP) Valve Catalogue1
jejujung547 visualizações
InspectionSamplingProceduresFineCoarseAggregates.pdfInspectionSamplingProceduresFineCoarseAggregates.pdf
InspectionSamplingProceduresFineCoarseAggregates.pdf
RiSovannaphumi17 visualizações
VAC-VBS-Gas-Permeability-TesterVAC-VBS-Gas-Permeability-Tester
VAC-VBS-Gas-Permeability-Tester
Labthink International,Inc.136 visualizações

Último(20)

Salvation a Work of GodSalvation a Work of God
Salvation a Work of God
Central Church of Christ18 visualizações
Thanks Giving Encouragement Wednesday.pptxThanks Giving Encouragement Wednesday.pptx
Thanks Giving Encouragement Wednesday.pptx
FamilyWorshipCenterD10 visualizações
CitSciOz MOUA Inspiring Change Through ArtCitSciOz MOUA Inspiring Change Through Art
CitSciOz MOUA Inspiring Change Through Art
Christian Bartens39 visualizações
SOA PPT ON SEA TURTLES.pptxSOA PPT ON SEA TURTLES.pptx
SOA PPT ON SEA TURTLES.pptx
EuniceOseiYeboah8 visualizações
Prospectus (1).pdfProspectus (1).pdf
Prospectus (1).pdf
PancrazioScalambrino14 visualizações
Speaking with confidence-converted.pdfSpeaking with confidence-converted.pdf
Speaking with confidence-converted.pdf
Abdul salam 16 visualizações
Transformers for time seriesTransformers for time series
Transformers for time series
EzeLanza5 visualizações
BLogSite (Web Programming) (1).pdfBLogSite (Web Programming) (1).pdf
BLogSite (Web Programming) (1).pdf
Fiverr10 visualizações

PPT on Mdpe inspection.pptx

  • 2. SCOPE IS 14885 covers the requirements for polyethylene pipe from dia. 16 mm to 630 mm with SDR 9,11,14 and 17.6 and in material grade PE-80 & PE- 100. • Raw Material • Inspection Raw material inspection In Process Inspection Final Inspection
  • 3. RAW MATERIAL CRP 100 Orange - CRP 100 orange is a high density polyethylene, The product is used for PE 100 and provides excellent stress crack resistance properties (ESCR) with very good long term hydrostatic strength. PE 100 XSC50 - It is a high performance hexene based orange compound, with a MRS 10 MPa. Eltex TUB 125 N2025- Eltex TUB 125 N2025 is a high-density polyethylene copolymer designed for the extrusion of pipes for gas applications. HE3492 LSH- It is used to ensure excellent long-term thermal stability and UV-resistance.
  • 4. INSPECTION •RAW MATERIAL INSPECTION •IN PROCESS INSPECTION •FINAL INSPECTION
  • 5. RAW MATERIAL INSPECTION •Density Test •Melt Flow Rate •Thermal Stability (OIT) •Pigment Dispersion •Volatile Matter Content
  • 6. DENSITY IS 14885, CL.-8.3, IS 7328, ANNEX-A • The density is determine by the buoyancy method by finding the mass in air and mass in butyl acetate. • Apparatus- Analytical balance, butyl acetate, hydrometer, beaker • Test sample- Weight- 50gm • Calculation – Density of PE (KG/M³) = a1*ρ*100/(a1-a2) a1 - Mass of specimen in air (gm) a2- Mass of specimen in butyl acetate (gm) ρ- Density of butyl acetate (0.877 KG/M³) • Density of butyl acetate determined by hydrometer. Density of pe should be ≥928.4 KG/M³ @23℃ & ≥ 𝟗𝟑𝟎 KG/M³ @27℃.
  • 8. MELT FLOW RATE (MFR) (IS 14885, CL.- 8.4, IS 2530) • Melt Flow Rate measures the rate of extrusion of thermoplastics through MFT at given temperature and load. • It provides measuring flow of a melted material which can be used to differentiate grades of pipes. • Sample size – 5 gm. @190℃ , min. 3 nos. sample required Weight (Load) – 5kg. • Calculation- MFR=m*600/t for gm/10 min. m - avg. mass of minimum 3 nos. sample. t - cut off time (240 sec.) • MFR of the compound material shall be ±20%.
  • 10. Thermal Stability (OIT) (IS 14885, CL.-8.5, ANNEX-D) OIT (oxidation induction time) is a type of test/method to measures the level of thermal stabilization or oxidation induction time of the pe material. The time between melting and the decomposition is measured. The atmosphere is nitrogen up to melting and then oxygen. - For long term strength - Stability of material - For electrofusion jointing w.r.t. temperature. Sample size- 15 mg Test temperature - 200℃ Gas flow of N2 & O2 – 50CM³/min. Thermal analyser equipment used for this test OIT ≥ 𝟐𝟎 𝑴𝑰𝑵𝑼𝑻𝑬𝑺 @𝟐𝟎𝟎℃
  • 11. PIGMENT DISPERSION (IS 14885, CL.- 5.4, ANNEX-E) The test is perform to check the proper dispersion in PE material. Apparatus- Microscope of at X 100 linear magnification. Microtome Hot plate Test specimen- Six test pieces shall be taken from different parts of the cross-section. Thickness & Area of specimen- 10𝜇𝑚 to 20𝜇𝑚 & 7 mm² Weight – 5 mg Principle- A microtomed section of material is examined by transmitted light at a magnification of X 100 and compared against standard photomicrographs. Acceptance- The grading should be ≤ 3.
  • 13. Volatile matter content (IS 14885, CL.- 8.6, ANNEX-H) • Volatile matter is an unstable material. Volatile matter tends to not remain in one state and will rapidly transition to another state, or vaporize, when the right conditions are met. • The volatile content is determined as the loss of mass of a sample, which has been put in a drying oven. • Calculation – V=(P1-P2)10^6/(P1-P0) V- volatile matter content (mg/kg) P0- weight of empty weighing cup (dia. 35mm) in gm. P1- weight of weighing cup & sample P2- weight of weighing cup and sample after 1 hr @105℃ Sample size- 25 gm. Volatile matter content should be ≤ 𝟑𝟓𝟎 𝒎𝒈 𝒌𝒈
  • 14. In Process Inspection • Colour • Finish Of Pipe • Outside Diameter • Wall Thickness • Ovality • Marking • Length
  • 15. Colour The colour of the pipes shall be yellow when manufactured from PE-80 grade and orange from PE- 1OOgrade. Colour coding confirm with BS 5252 PE 100 – CODE 08 E 55 PE 80 – CODE 08 E 53
  • 16. Finish of Pipe • Smooth • Clean • Free from grooves • The ends shall be cleanly cut and shall be square with axis. • Considerable “Out of Square Tolerance of End”- 2mm for 16 to 90mm dia. 3mm for 90 to 140mm dia. 4mm for 140 to 200mm dia.
  • 18. Wall thickness • Negative tolerance should not allowed during inspection of pipe. • Ball ended micrometer used to check the thickness. • Acceptable plus tolerance- Table 4 & 5 of IS 14885
  • 21. Marking • All pipes shall be permanently marked along their length with a legend, which shall be impressed to a depth of not more than 0.2 mm. • Marking details shall be formed on the pipe in such away that the marking does not initiate cracks or other type of failure. • The embossing for yellow/ orange pipe shall have black Colour. The height of the character shall be uniform and at least 3 mm for ≤ 90𝑚𝑚 & 5 mm for ≥90mm. • The legend shall be repeated at intervals of 1 m . • Manufacturer’s name, Designation and Batch or lot number. • Each pipe may also be marked with the Standard Mark.
  • 23. Length • PE 100 DN 20MM SDR 11 – 200 MTRS. • PE 100 DN 32MM SDR 11 – 200 MTRS. • PE 100 DN 63 MM SDR 11 – 100 MTRS. • PE 100 DN 125 MM SDR 17.6- 50 MTRS.
  • 24. Final Inspection •Hydraulic Pressure Resistance Test •Reversion •Tensile test (Tensile Strength at Yield & Elongation at Break) •Resistance to weathering (Exposure to sunlight) •Supply, Packaging, Handling & Transportation
  • 25. Hydraulic Pressure Resistance Test (IS 14885, CL. 8.1, ANNEX-A&B, TABLE -7) • When specimen subjected to internal pressure as per given procedure, sample shall show no sign of swelling, leakage, burst or any type of physical damage. • TEST SPECIMAN – Sample taken after 24 hrs. of manufacturing. Size- 10*OD (250mm to 750mm). For < ∅63𝑚𝑚 → @80℃ for 165 hrs.→ 5.5 Mpa (induced stress) For ≥ ∅63𝑚𝑚 → @80℃ for 165 hrs.→ 4.6 Mpa (induced stress) • Calculation – Test Pressure (in MPA)=2 𝜎𝑠 𝑑−𝑠 𝜎 − 𝑖𝑛𝑑𝑢𝑠𝑒𝑑 𝑠𝑡𝑟𝑒𝑠𝑠 𝑇𝑎𝑏𝑙𝑒 − 7 s – minimum wall thickness d – outside dia. Conclusion - sample shall show no sign of swelling, leakage, burst Or any Damage during test perform @ above given condition https://www.youtube.com/watch?v=0qD05rWK39g
  • 26. Hot water bath Test Sample
  • 28. REVERSION (Shrinkage Or Expansion) (IS 14885, CL. 8.2) • The test is performed to check the shrinkage or expansion of pipe. • Apparatus- Hot air circulating oven (@110℃) Vernier caliper Glass plate Talcum powder • Test specimen- Size- 200mm for ≤ 200𝑚𝑚 & Axial arc of 200mm for ≥ 200𝑚𝑚 No. of sample – ≥ 3 • Calculation- Reversion (%)= (Li-Lf)*100/Li • Conclusion- Value should be in b/w of +3 and -3 in percentage.
  • 30. Tensile test- (IS 14885, CL. 8.7, 8.1, CL.-06 OF IS 2530) • Tensile yield strength & Elongation at break test of mdpe. • Test speciman- Use a sufficiently long piece of pipe, and divide its circumference into a certain number of sectors with an arc length of 150 mm. For thickness of specimen- < 5𝑚𝑚 → @ 23°C & 100 mm/min ≥ 5𝑚𝑚 → @ 23°C & 25 mm/min • Apparatus – Universal tensile tester • Procedure- The test pieces shall be conditioned for two hours in air or one hour in water so that it is at a temperature of 27°C immediately before test. • Acceptance- Tensile yield strength 15 Mpa Elongation at break 350 percent, Min
  • 33. Resistance to weathering (Exposure to sunlight) (IS 14885, CL.-8.8, ANNEX-F) • Test specimen – Length – 1 mtr. 0.2 mm upper layer of specimen shall be remove before testing. • Time period – Sample shall be exposed for a period of six months. The size of the apparatus and the distance between the specimens shall be such that no shadows fall across the specimens for the period of at least 8 h during which the sun is normally the strongest. • Acceptance- Elongation as per 8.7.1 Hydraulic characteristics as per 8.1 Thermal stability to oxidation as per 8.5
  • 34. Supply, Packaging, Handling & Transportation (IS 14885, CL. 11, ANNEX-K) • SUPPLY-  The polyethylene pipes shall be supplied as straight length either independent or bundled together.  Pipe ends shall be cleanly cut, square with the axis of pipe and with appropriate end caps • Coils- Polyethylene pipes may be coiled or packed on drums. Large diameter coils with d> 90 mm should be stored flat or vertically. • Coil Dimension and Winding Temperature- Size Minimum internal dia Max. external coil dia 20/25 mm 0.6 m 3.2 m 32 mm 0.7 m 3.2 m 63 mm 1.3 m 3.2 m 125 mm 2.5 m 3.2 m Maximum external surface temperature at time of coiling- 35℃ • All the coils shall be wrapped with PP woven sack & PE film.